FePt thin films with a thickness of 30 nm were deposited by dc magnetron sputtering at room temperature onto SiO2(100 nm)/Si(100) substrates. These films were post-annealed in a temperature range of 500 °C to 900 °C for 30 s in three different atmospheres—N2, Ar, and forming gas (Ar+H2 (3 vol. %)). Irrespective of the annealing atmosphere, the chemically ordered L10 FePt phase has formed after annealing at 500 °C. Higher annealing temperatures in N2 or Ar atmosphere resulted in a strong increase in grain size and surface roughness but also in the appearance of a pronounced (001) texture in the FePt films. However, these films show the presence of iron oxide. In contrast, annealing in forming gas atmosphere suppressed the oxidation process and resulted in a reduced grain size and lower surface roughness. However, no (001)—but a strong (111)—texture was obtained after annealing at 700 °C, which might be related to the reduced unit cell tetragonality and incorporation of hydrogen to the FePt lattice. Thus, this study clearly demonstrates that the oxygen/hydrogen content plays an important role in controlling the crystallographic orientation during post-annealing.
Pt /Fe and Pt /Au /Fe layered films were deposited at room temperature by dc magnetron sputtering on Al 2 O 3 (0 0 0 1) single crystalline substrates and heat treated in vacuum at 330 °C with different durations (up to 62 h). It is shown by secondary neutral mass spectrometry depth profiling and x-ray diffraction that the introduction of an additional Au layer between Pt /Fe layers leads to enhanced intermixing and formation of the partially chemically ordered L 1 0 FePt phase. The underlying diffusion processes can be explained by the grain boundary diffusion induced reaction layer formation mechanism. During the solid state reaction between Pt and Fe, the Au layer moves towards the substrate interface replacing the Fe layer. This was explained by the much faster diffusion of Fe, as compared to Pt, along the grain boundaries in Au. Enhancement of the process and formation of the ordered FePt phase in the presence of the Au intermediate layer were interpreted by the effect of stress accumulation during the grain boundary reactions: the disordered FePt phase formed initially at different Au and Pt grain boundaries can experience appropriate compressive stress along the {1 0 0} directions, which can initiate the formation of the chemically ordered L 1 0 FePt phase.
Pt/Fe and Pt/Ag/Fe layered films were deposited by DC magnetron sputtering on MgO(001), SrTiO3(001), and Al2O3(0001) single crystalline substrates at room temperature. The films were post-annealed between 623 K and 1173 K for 30 s in flowing N2 atmosphere. The onset of the L10-FePt phase formation in films deposited on MgO(001) and SrTiO3(001) substrates was observed after annealing between 773 and 873 K, while chemical L10 ordering sets in for Pt/Fe bilayers on Al2O3(0001) at lower temperatures accompanied by strong (001)-texture. It is concluded that elastic stress, arising from the difference in thermal expansion coefficients between film and substrate, promotes ordering and texture formation.
27 March 2015 in Journal of Physics D: Applied Physics
Depth profiles of tri-layered Fe(15 nm)/Ag(10 nm)/Pt(15 nm)/SiO 2 (100 nm)/Si(1 0 0) and bi-layered Fe 50 Pt 50 (15 nm)/Ag(7.5 nm)/SiO 2 (100 nm)/Si(1 0 0) thin films after different heat treatments were investigated by secondary neutral mass spectrometry. Isotherm annealing of the tri-layered samples was carried out between 245 and 390 °C up to several hours, while isochrone thermal annealing was performed between 600 and 900 °C for 30 s. Composition profiles, obtained after isotherm heat treatment, show that initially there was a strong intermixing between Ag and Pt, resulting most likely in the formation of an Ag x Pt
1−
x reaction layer. Furthermore, the intermixing process was much faster in the Ag layer accompanied by the segregation of Ag to the substrate/Pt interface. Later on the Pt, which diffused through the Ag layer, started to penetrate into the Fe grain boundaries. This process led to the formation of the FePt reaction product. At the same time as the Pt diffused into the Fe layer, reducing the amount of Pt in the Ag x Pt
1−
x layer, the Ag appeared to ‘move’ towards the substrate. Finally, an almost fully homogeneous FePt alloy layer formed with some FePt present in the grain boundaries of the remaining Ag. This behavior was compared to both types of samples subjected to isochrone thermal annealing. High temperature treatments resulted in similar results and eventually in the formation of a homogeneous L1 0 ordered FePt alloy with randomly distributed Ag in the grain boundaries and at the free surface.