This study aims to clarify how a solution’s pH can influence the corrosion and formation of surface films on the AZ31 Mg alloy in aqueous solutions containing sulfate ions. The corrosion and surface film formation behaviors were examined using in situ observation, open-circuit potential (OCP) transient, weight change measurement and electrochemical impedance spectroscopy (EIS). The morphologies of the surface films were analyzed via metal/insulator/metal (MIM) coloring and FESEM. The findings show that at pH 2, severe corrosion occurred together with rapid hydrogen evolution and formation of a highly porous surface film with numerous cracks. However, at pH 3, the corrosion rate dropped significantly and remarkably low corrosion rates were observed at pH 4 and 10. At pH 11 and 12, weight gains were noticed, suggesting the growth of surface films on the AZ31 Mg alloy. Flake-like films formed at pH 12, while needle-like structures were present between pH 3 and 11. Impedance measurements revealed increased impedance at higher pH of sulfate-ion-containing solutions. Higher impedance was related to the formation of denser surface films on the AZ31 Mg alloy. In addition, the films displayed metal/insulator/metal (MIM) colors via Au coating above pH 4, indicating uniform film thickness despite the presence of needle-like or flake-like structures.
This work demonstrates the corrosion behavior of the AZ31 Mg alloy as a function of an immersion time of 48 h in 0.1 M HCl, H2SO4, H3PO4 and HF solutions, in which pH was adjusted to 6 to exclude the contribution of hydrogen ions (H+) and hydroxide ions (OH−). In situ observations, open circuit potential (OCP), weight changes and AC impedance measurements were performed with an immersion time of 48 h and the morphologies and chemical compositions of the surface products after 48 h of immersion were analyzed by SEM, EDS and XPS. In the chloride ion (Cl−)-containing solution, the corrosion of the AZ31 Mg alloy initiated locally and propagated discontinuously over the surface with immersion time. The OCP value of the AZ31 Mg alloy showed an initial increase from −1.51 VAg/AgCl to −1.47 VAg/AgCl after about 5 h of immersion and then a decrease to −1.51 VAg/AgCl due to corrosion initiation. In the F−-containing solution, after 48 h of immersion, the OCP showed an extremely large value of −0.6 VAg/AgCl, while the relatively lower values of −1.52 VAg/AgCl, −1.59 VAg/AgCl were seen in the solutions containing SO42− and PO43, respectively. In the sulfate ion (SO42−)-containing neutral aqueous solution, needle-like surface films were formed and there were no changes in the weight of the AZ31 Mg alloy with immersion time. In the phosphate ion (PO43−)-containing neutral aqueous solution, a vigorous gas evolution occurred, together with the formation of black surface films with cracks, and a high corrosion rate of −13.8018 × 10−3 g·cm−2·day−1 was obtained. In the fluoride ion (F−)-containing neutral aqueous solution, a surface film with crystalline grains of MgF2 was formed and the weight of the AZ31 Mg alloy increased continuously with immersion time. In conclusion, the corrosion of the AZ31 Mg alloy occurred uniformly in neutral phosphate solution but locally in chloride solution. No corrosion was observed in either the neutral sulfate or fluoride solutions.
Tribological behaviors of the plasma electrolytic oxidation (PEO)-treated Al1050 alloy surface without and with Ni-P deposits was examined by analyzing of the width of abrasion groove, weight loss, friction coefficient and composition at the wear track after a 100 m ball-on-disc test. The surface color, surface and cross-sectional morphologies and surface roughness (Ra) were also investigated to explain different wear behaviors of PEO films without and with Ni-P deposit. After the 100 m ball-on-disc test, a circular abrasion groove with relatively large width and shallow depth was formed when Ni-P particles cover the top surface of PEO films, but a relatively narrow and deep circular abrasion groove was formed on the Ni-P layer-covered PEO film surface. Iron was only detected at the wear track of 5 and 10 μm PEO films without Ni-P deposit, suggesting that the steel ball is worn out by the PEO films but not by the Ni-P deposit. An extremely large amount of weight loss was obtained from the Ni-P layer-covered PEO film surface, which could be related to the high density and low hardness of the Ni-P layer.