Cracking is one of the main distresses in asphalt pavement. At present, few studies have been conducted on the cracking performance of asphalt mixtures from the field due to the difficulty of sample collection. Therefore, this study aims to assess the cracking resistance of in-service asphalt pavement at intermediate temperature using a large number of field cores in Jiangsu province, China. A semi-circular bending (SCB) test at 25 °C was conducted on field-cored samples covering three asphalt layers from 16 in-service road sections that represent a combination of influencing factors, including air void, mixture type, service age, cumulative number of equivalent single-axle loads (ESALs), and overload rate. The flexibility index (FI) and tensile strength were calculated from the experimental data as cracking performance evaluation indices. According to the analysis of variance results, at the top layer, ESALs and service age had a strong influence on cracking resistance. The decline rate of FI became slower with increasing ESALs. The most rapid decline in crack resistance with service age occurred on medium-traffic-level sections that served for over 14 years. At the middle layer, the overload rate replaced service age as a significant factor for FI. At the bottom layer, the air void was the only significant factor affecting the cracking resistance. In general, as the depth of layer increased, the effect of traffic load and service age decreased, whereas the effect of material properties increased. In addition, the FI and tensile strength were more sensitive to traffic load and air void, respectively.
With the increasing service life of asphalt pavements, fatigue cracking has become a typical distress that significantly affects the structural lifespan of in-service asphalt pavements. To address the issues of high variability in laboratory fatigue tests and the poor correlation between test results and actual pavement cracking conditions, this study collected field core samples from in-service highways with varying degrees of cracking. The study employed push-pull fatigue tests on asphalt mixtures and linear amplitude sweep tests on extracted and recovered asphalt to evaluate fatigue performance. Quantitative relationships between transverse crack spacing and fatigue indices were established. With the inclusion of laboratory-compacted asphalt mixtures, the relationship between transverse crack spacing and the average pseudo-stiffness degradation rates was well described by a logarithmic function (R2 = 0.928), while the apparent damage capacity achieved a stronger correlation (R2 = 0.945). The findings demonstrate that the push-pull fatigue test, based on a viscoelastic continuum damage model, shows high stability and repeatability, with the coefficients of variation for the indices consistently below 11%. Compared to the average pseudo-stiffness degradation rates, the apparent damage capacity demonstrates better discriminative capability as an evaluation index for the intermediate-temperature fatigue performance of asphalt mixtures. The fatigue life from linear amplitude sweep tests on extracted and recovered asphalt from core samples shows a high degree of consistency with the patterns observed in various parameters of push-pull fatigue tests. The findings confirm the reliability of the push-pull fatigue test for evaluating intermediate-temperature fatigue performance of asphalt mixtures and provide the necessary theoretical support for establishing a fatigue performance evaluation system for in-service asphalt pavements.