Microstructure evolutions and mechanical properties of a commercially pure titanium (CP-Ti, grade 2) during multi-pass rotary-die equal-channel angular pressing (RD-ECAP) and cold rolling (CR) were systematically investigated in this work, to achieve comprehensive property for faster industrial applications. The obtained results showed that the grain size of CP-Ti decreased from 80 μm of as-received stage to 500 nm and 310 nm after four passes and eight passes of ECAP, respectively. Moreover, abundant dislocations were observed in ECAP samples. After subsequent cold rolling, the grain size of ECAPed CP-Ti was further refined to 120 nm and 90 nm, suggesting a good refining effect by combination of ECAP and CR. XRD (X-ray diffractometer) analysis and TEM (transmission electron microscope) observations indicated that the dislocation density increased remarkably after subsequent CR processing. Room temperature tensile tests showed that CP-Ti after ECAP + CR exhibited the best combination of strength and ductility, with ultimate tensile strength and fracture strain reaching 920 MPa and 20%. The high strength of this deformed CP-Ti originated mainly from refined grains and high density of dislocations, while the good ductility could be attributed to the improved homogeneity of UFG (ultra-fine grained) microstructure. Thus, a high strength and ductility ultra-fine grained CP-Ti was successfully prepared via ECAP plus CR.
Pure titanium was efficiently processed up to four passes at 420 °C by rotary-die equal-channel angular pressing (RD-ECAP). The deformation structure and mechanical properties of pure titanium with various RD-ECAP passes were subsequently investigated. Microstructure evolution revealed that plastic deformation was accommodated mainly by twins during the first and second passes, while the predominant deformation mechanism was dislocation slip during the third and fourth passes. { } twins were detected in the first pass, and { } twins occurred in the second pass of RD-ECAP. The ultimate tensile strength of pure titanium increased from 450 MPa in the as-received state to 627 MPa with a fracture elongation of 29% after four passes of RD-ECAP.
Industrial pure titanium was processed through 1–4 passes by equal-channel angular pressing (ECAP), and the processed samples were subsequently short-term annealed for 15 min at 300 °C, to achieve better mechanical properties for industrial applications. The microstructure was analyzed using TEM, EBSD, and XRD observations. The mechanical properties were studied through tensile testing. The TEM and EBSD results showed that the grain size of industrial pure titanium was refined to approximately 420 nm after four passes of ECAP processing, with very little grain growth after annealing. The XRD analysis proved the enhanced basal texture in the subsequent annealed samples. Tensile tests indicated that the strength of the processed sample increased with more ECAP passes and was improved by 39% after four passes compared with the as-received state; in addition, the low-temperature short-term annealing resulted in a further strengthening phenomenon. It was concluded that the strengthening after annealing in industrial pure titanium was likely due to the improved basal texture, resulting in texture strengthening.
Grains of commercially pure titanium (CP-Ti) can be refined via rotary-die equal-channel angular pressing (RD-ECAP) to meet higher application requirements. However, the grain refinement mechanism of CP-Ti during RD-ECAP has not been fully studied. Herein, CP-Ti was processed up to four passes by RD-ECAP to obtain an ultrafine-grained structure. The microstructure evolution, refinement mechanism, and dynamic recrystallization (DRX) behavior was investigated by TEM and EBSD analysis. The results revealed that after two passes, banded structures with numerous LAGBs inside were detected, while after four passes, most grains were equiaxed with HAGBs and the average grain size was about 0.5 μm. The fraction of HAGBs reached 78.6% for the four-pass sample, which was higher than that of two-pass sample. The fraction of deformed grains declined and the proportion of recrystallized grains increased as the pass number increased from two to four. The misorientation gradient analysis showed that subgrains with LAGBs evolved into new grains with HAGBs gradually to generate ultrafine grains. The refinement mechanism of CP-Ti during RD-ECAP can be concluded as continuous DRX (CDRX). In addition, the relationship between DRX type and the processing conditions as well as stacking fault energies (SFEs) of metals was innovatively explored, providing a new approach for predicting microstructure.