In the present study, a powder of Ti-18Zr-15Nb biomedical alloy with spongy morphology and with more than 95% vol. of β-Ti was obtained by reducing the constituent oxides with calcium hydride. The influence of the synthesis temperature, the exposure time, and the density of the charge (TiO2 + ZrO2 + Nb2O5 + CaH2) on the mechanism and kinetics of the calcium hydride synthesis of the Ti-18Zr-15Nb β-alloy was studied. Temperature and exposure time were established as crucial parameters with the help of regression analysis. Moreover, the correlation between the homogeneity of the powder obtained and the lattice microstrain of β-Ti is shown. As a result, temperatures above 1200 °C and an exposure time longer than 12 h are required to obtain a Ti-18Zr-15Nb powder with a single β-phase structure and uniformly distributed elements. The analysis of β-phase growth kinetics revealed that the formation of β-Ti occurs due to the solid-state diffusion interaction between Ti, Nb, and Zr under the calcium hydride reduction of TiO2 + ZrO2 + Nb2O5, and the spongy morphology of reduced α-Ti is inherited by the β-phase. Thus, the results obtained provide a promising approach for manufacturing biocompatible porous implants from β-Ti alloys that are believed to be attractive candidates for biomedical applications. Moreover, the current study develops and deepens the theory and practical aspects of the metallothermic synthesis of metallic materials and can be compelling to specialists in powder metallurgy.
The effects of severe plastic deformation on NiTi alloys’ structure and properties have been extensively studied over the past decades. However, there is a notable lack of systematic data regarding the impact of industrial hot deformation techniques on these alloys. This gap arises from challenges in manufacturing processes related to the unevenness of ingots produced by casting technologies. This study investigates the effects of hot rotary swaging, extrusion, and radial shear rolling on the martensitic transformation, shape memory effect, superelasticity, and damping capacity of NiTi Ni-rich alloys fabricated through powder metallurgy. The properties were investigated under torsional load on wires prepared by spark eroding from deformed rods. Our findings indicate that samples after rolling and extrusion exhibit a superelastic strain of 14 ± 0.5% attributed to a high yield stress of approximately 600–800 MPa and torsional testing providing the material to be fully involved in recovery process. Samples after rolling and swaging demonstrate a high level of reversible strain with a one-way shape memory effect ranging from 5 to 7%. Conversely, extrusion, due to the inhomogeneity of resulting workpieces, induces a complex, multi-stage martensitic transformation that undermines the shape memory effect. Furthermore, all deformation methods except extrusion contribute to increased alloy homogeneity, resulting in a narrower temperature range for martensitic transformations. Rotary swaging notably increases the height of an internal friction peak from 0.015 to 0.045 compared to the undeformed material, whereas rolling gives the lowest value of 0.012 among others. This study provides valuable insights into how hot thermomechanical processing influences the properties of NiTi alloys and shows that powder metallurgy combined with hot deformation can be considered an alternative approach for achieving high functional properties of these alloys.
—The influence of various schemes of thermomechanical treatment (TMT) on the structure and properties of two sintered nickel-rich binary TiNi powder alloys is shown. TMT is found to decrease the average grain size and to increase the strength characteristics, the alloy density, and the plasticity relative to the initial sintered state. The influence of TMT on the phase composition of the alloy is detected by X-ray diffraction. TMT is shown to promote the formation of the triclinic R-martensite or strain aging with the precipitation of the Ti2Ni3 phase.
The authors studied the structure, a phase composition, mechanical and functional properties of a TiNi binary powder alloy (Ni = 55.5% (wt.)) after cross rolling at 900 oC with a degree of true strain of ε = 1.5. It is shown that after cross rolling at ε = 1.5 the structure contained R-martensite amounting to 5% or less. Due to lower rolling temperature, the dynamic recrystallization develops in some volume, and only a share of grains is in a polygonized and recrystallized state. The average grain size is dav = 34±2 μm, which is significantly lower than after a preceding deformation stage (ε = 0.8, dav = 64 ± 2 μm). Variations in a grain size occur in center and surface layers of rolled rods. However, such variations in a grain size do not influence microhardness across the sample section. As a result of the deformation at ε = 1.5, axial porosity decreases, entailing an increase in the alloy density up to 6.4 g/cm3. The decreased axial porosity and grain refinement contributed to an increase in ductility up to a required level (δ >10%). Thus, a set of mechanical properties of TiNi after cross rolling at a strain degree of ε = 1.5 satisfies requirements of specifications TU 1-809-394–84 for alloy grade TN1. It is shown that after rolling a TiNi powder alloy is characterized by its high damping capacity in a temperature range of a martensite transformation. When carrying out tests, this alloy in austenite state shows superelasticity, while during tests in martensite-austenite state — superelasticity and shape memory effect. The studies on the effect of preliminary torsional deformation on shape memory properties showed that the shape of wire samples was fully restored up to γtor = 14%, then an unrestored part of deformation occurs due to an unreversible sliding effect.
The refractory Laves phase TaCr2 of two compositions (series) was synthesized by the metallothermal (hydride-calcium) method from oxide raw materials (Cr2O3 + Ta2O5). The synthesis temperature was 1200 oC, while the excess of the reducing agent CaH2 was varied relative to the theoretically required for the complete reduction of oxides. It is shown that regardless of the excess of the reducing agent or in its complete absence, the resulting powders have the required chemical composition (composition 1: calculated Cr content — 37.38% (wt.), actual — 37.50±0.85% (wt.); composition 2: calculated Cr content — 35.30% (wt.), actual — 35.38±0.31% (wt.)). No significant losses of Cr and Ta were observed during the synthesis of the Laves phase under the conditions of hydride-calcium reduction of Cr2O3 and Ta2O5. All prepared powders contained ~ 0.25% (wt.) oxygen and 0.025% (wt.) calcium. This is a good result for experimental batches first obtained by this method. Powders of the first series (composition 1), regardless of the excess of CaH2, contained no less than 85% (wt.) of the TaCr2 phase of the С15 type and ~ 10% (wt.) of the Cr(Ta) solid solution. However, when the excess of the reducing agent was >50 wt%, a high-temperature modification of the TaCr2 phase with a C14-type hexagonal lattice came in sight. The same picture was observed in the second series of experiments (composition 2). In all cases, the amount of the C14 type TaCr2 phase did not exceed 5% (wt.). Powders of composition 2 contained no less than 90% (wt.) of the C15 type TaCr2 phase or 95% (wt.), if there were two modifications C15 + C14. Depending on the excess of the CaH2 reductant, the alloys contained small amounts of Cr(Ta) or Ta2H hydride. In both series, the powder particles had a finely dispersed spongy structure; large particles of regular shape were present in an insignificant amount. This work was carried out with financial support of the government of the Tula region (grant for work in the field of science and technology No. DS / 161 dated October 29, 2020).
1 September 2020 in Inorganic Materials: Applied Research
The effect of consolidation and thermal treatment on the structure, local chemical composition, and martensite transformation temperatures of the Ti28Ni50Hf22 powder alloy is studied. It is shown that, in the powder state, the alloy is characterized by an inhomogeneous distribution of Ti and Hf in the matrix, whose concentration spread may reach 27 at %. Vacuum sintering and homogenizing annealing lead to equalization of the chemical composition. During powder sintering, the spread of Ti and Hf concentrations reduces from 27 to 2 at %. Subsequent vacuum annealing at a temperature of 1000°C for 4 h for a sintered sample additionally reduces the spread of concentrations from 4 to 2 at %, while the increase in the annealing duration from 4 to 16 h does not affect the uniformity of the element distribution. It is established that, at a large inhomogeneity of the chemical composition, the differential scanning calorimetry (DSC) methods fail to record the occurrence of martensitic transformation in the melt. However, homogenization of the alloy leads to the appearance of endothermic peaks on the DSC curve upon heating, as well as to narrowing of the interval of reverse martensitic transformation.