The eutectic high entropy alloy Nb0.73CoCrFeNi2.1 was manufactured by means of arc smelting and the obtained ingots were cut into 300-μm-thick foils, which were used as filler alloys to braze Crofer 22 APU to Hf-metallized yttria-stabilized zirconia (3YSZ). The brazing process was conducted in a vacuum furnace at 1200 °C for 5 min at a vacuum of 4.3·10–4 mbar. In order to minimize the intense diffusion and erosion of the steel substrate, a heating and cooling rate of 50 K/min was applied. Sound joints without any pores or flaws were obtained. The microstructure of the joints consisted of an HfO2 reaction layer at the ceramic interface and the same eutectic structure consisting of a Laves phase and a solid solution that was already detected in the smelted foil. The average hardness of the microstructure in the joint seam amounted to 352 ± 17 HV0.01 and the joints reached strength values up to 97 ± 7 MPa while the fracture area was always located at the ceramic interface in the HfO2 layer. Comparable joints, with AgCuTi3 as filler metal, brazed at 920 °C, only reached a shear strength of ~ 52 ± 2 MPa.
29 August 2023 in Journal of Materials Research and Technology
Vacuum brazing is a black box process, so component distortion that occurs during the heat treatment is difficult to prove experimentally. Thus, a novel FE-model was developed in ANSYS Workbench to calculate the time and location resolved component deformation of AISI 316L/B-Ni2 brazing assemblies. In this regard, a new method of radiation and contact modeling was developed that enabled a significant reduction of the calculation times and solved the convergence issue for simulating the distortion of large-scale, thin components. The results showed that the component deformation during heating can be easily kept in the elastic range and can be almost completely eliminated by using a geometry-dependent soaking time. In contrast to this, high cooling rates were found to result in thermally induced stresses well above the elastic yield limit, causing significant component deformation. With further cooling, the deformation decreases significantly, but it depends on the initial stress state, the geometry, and the cooling rate whether the deformation can be completely leveled out during the shrinkage of the component. Thus, the initially high cooling rates were identified to be responsible for the final distortion. Furthermore, this was highly affected by the local position in the heating chamber. The simulation results were used to design a fixture for vertical positioning, which reduced the max. temperature difference in the brazing assembly from 141 to 79 °C, the max. interim distortion from 275 to 31 µm, and the final distortion from 14 to 8 µm.
This paper investigates if the polar groups induced by a plasma treatment can increase the lap shear strength of laser-joined metal and plastic hybrids. Optimal laser joining parameters for cold-rolled AISI304–polyamide 6.6 and sandblasted AISI304–polypropylene hybrids were developed at 2.85 MPa and 4.22 MPa, respectively. The surface free energy was doubled for all used plasma gases to a value of ca. 80 mN m−1 at 180 s. The plasma-treated samples were joined and tested. The arithmetic means of the plasma-treated hybrids’ lap shear strength with polyamide 6.6 varied slightly, but all measured values were within the range of the untreated samples. Residue on the sheared metal samples indicated covalent bonds between AISI304 and polyamide 6.6. The lap shear strengths of the plasma-treated polypropylene hybrids were significantly reduced between −30.8% and −53.3%, depending on the used plasma gas. This was attributed to the over-aging and development of low-molecular-weight oxidized materials, which led to a weak boundary layer. No residue of polypropylene was found on treated or untreated lap shear samples. No correlation between the surface free energy and lap shear strength could be found.
The strength of laser joined metal and plastic hybrids is based purely on adhesion. Unpolar plastics like polypropylene depend solely on the mechanical adhesion while polar plastics like polyamide 6.6 develop covalent bonds with the metal. In this research the influence of different surface metallizations on the lap shear strength of laser joined hybrids was investigated. Sandblasted AISI 304 was used as base metal and reference. Aluminum and titanium coatings were deposited by the means of Arc-PVD. Polypropylene and polyamide 6.6 were utilized as polar und unpolar plastics. The lap shear strength of all hybrids with polyamide 6.6 was higher than the polypropylene samples. For all investigated variations of the laser power, scanning speed and the cohesive and adhesive failure modes, the samples joined with the sandblasted AISI 304 showed the highest lap shear strength. The reduction in lap shear strength for the coated samples was due to the increased difference in thermal conductivity between the plastics and the coating materials. This lead to increased warping and residual stresses. It can be concluded that the thermal properties of the metallization in laser joined metal and plastic hybrids has a high impact on the lap shear strength.
This paper investigates if the polar groups induced by a plasma treatment can increase the lap shear strength of laser joined metal and plastic hybrids. Optimal laser joining parameters for cold-rolled AISI304 – Polyamide 6.6 and sandblasted AISI304 - Polypropylene hybrids are developed. The OWRK-method was utilized to identify the change in surface free energy of a low-pressure plasma treatment. Plasma treated samples were joined and tested. The fractured surfaces were investigated via light microscopy and SEM. The arithmetic means of the plasma treated hybrids lap shear strength with polyamide 6.6 varied slightly but all measured values were within the range of the untreated samples. The lap shear strengths of the polypropylene hybrids were significantly reduced. This was attributed to an overaging and the development of low molecular weight oxidized materials which lead to a weak boundary layer. No correlation between surface free energy and the lap shear strength could be found.