A mixture of abramis brama (freshwater bream), carassius carassius (crucian carp), and sander lucioperca (pike perch) scales was used for the preparation of fish scale powder containing constituents of organic and inorganic nature. The mixture of the mentioned fish scales was washed, dried, and ground for the preparation of fish scale powder. Vibration sieving was used to prepare fish scale powder enriched with inorganic components. According to thermal analysis data, this fish scale powder enriched with inorganic components included about 36.5 wt.% components removed when heating, primarily those of organic nature, and 63.5 wt.% mineral components. Inorganic powders consisting of hydroxyapatite and magnesium whitlockite were obtained via heat treatment of this fish scale powder at 800–1000 °C. Particles of these inorganic powders consisted of sintered grains with dimensions less than 100 nm after heat treatment at 800 °C, less than 200 nm after heat treatment at 900 °C, and 100–1000 nm after heat treatment at 1000 °C. Fish scale powder enriched with inorganic components as well as heat-treated inorganic powders consisting of hydroxyapatite and magnesium whitlockite can be recommended for the production of different materials, such as ceramics or composites.
Properties of composite materials with polymer matrix and inorganic filler are affected by preparation methods and starting components’ properties. For example, filler powder particle size distribution, phase composition and presence/absence of dopants can greatly affect properties of resulting composites. The present research attempts to clarify the influence of synthetic CaCO3 powder properties on alginate/CaCO3 composite material preparation process. Composite materials in the form of granules, networks and films were created from suspensions of synthetic powders of calcium carbonates CaCO3 in aqueous solutions of sodium alginate. Powders of calcium carbonates CaCO3 were synthesized from 0.5 M aqueous solutions of calcium chloride CaCl2 and aqueous solutions of potassium K2CO3 (at molar ratio Ca/CO3 = 1), sodium Na2CO3 (at molar ratio Ca/CO3 = 1), and ammonium (NH4)2CO3 (at molar ratios Ca/CO3 = 1 and Ca/CO3 = 0.5) carbonates. Phase composition of powder synthesized from CaCl2 and K2CO3 was presented by calcite. Phase composition of powders synthesized from other soluble carbonates included calcite and vaterite. The powder preparation protocol excluded the stage of synthesized powder washing for by-product removal. This preparation protocol provided preservation of reaction by-product in the synthesized powder at a very low level. The presence of NH4Cl as a reaction by-product even in small quantities can be taken as a reason for visually observed subsequences of cross-linking reaction at the stage of suspensions preparation. Aqueous solution of sodium alginate and suspensions containing powders synthesized from potassium K2CO3 and sodium Na2CO3 carbonates demonstrated similar dependence of viscosities from shear rate. The presence of (NH4)2CO3 in the powder synthesized at molar ratio Ca/CO3 = 0.5 was the reason for the lower viscosity of the suspension in comparison with suspensions loaded with powders containing KCl, NaCl and (NH4)2Cl as reaction by-products due to decomposition of unstable (NH4)2CO3 and gas phase formation. The presence of (NH4)2Cl in the powder synthesized at molar ratio Ca/CO3 = 1 in contrast was a reason for the highest viscosity suspension in comparison with those under investigation. Additionally, (NH4)2Cl presence in synthetic powders shows the ability to facilitate partial dissolution of CaCO3 providing a higher concentration of Ca2+ cations at the stage of suspension preparation, thus aiding the cross-linking process of alginate hydrogel. Granules, meshes and films were created via interaction of suspensions of calcium carbonates CaCO3 in aqueous solutions of sodium alginate with 0.25 M aqueous solutions of calcium chloride CaCl2 to provide the formation of matrix of composites via Ca-crosslinking of sodium alginate followed by washing and freeze drying under deep vacuum. The created composite materials in the form of granules, meshes and films based on Ca-cross-linked alginate and powders of synthetic calcium carbonate can be recommended for skin wound and bone defect treatment and drug delivery carriers.
Mixture of abramis brama (freshwater bream), carassius carassius (crucian carp), and sander lucioperca (pike perch) scales was used for the preparation of fish scale powder containing about 26.5 wt. % of removed when heating components preferably of organic nature, and 63.5 wt. % of mineral components. Fish scale powder enriched with inorganic components was prepared from washed, dried, and ground fish scale mixture using vibration sieving. Inorganic powders consisting of hydroxyapatite and magnesium whitlockite were obtained via heat treatment of this fish scale powder at 800-1000 oC. Particles of these inorganic powders consisted of sintered grains with dimensions less than 100 nm after heat treatment at 800 oC, less than 200 nm after heat treatment at 900 oC, and 100-500 nm after heat treatment at 1000 oC. Fish scale powder enriched with inorganic components as well as heat-treated inorganic powders consisting of hydroxyapatite and magnesium whitlockite can be recommended for the production of different materials such as ceramics or composites.
Powders with a phase composition including syngenite (K2Ca(SO4)2·H2O) and/or calcium sulfate dihydrate (gypsum, CaSO4·2H2O) were synthesized from the powder of calcium carbonate (CaCO3) and water solutions of potassium hydrosulfate (KHSO4) of various concentrations (0.5 M, 1 M, and 2 M). A molar ratio of starting salts, KHSO4/CaCO3 = 2, was used to provide the formation of syngenite (K2Ca(SO4)2·H2O). But when using a 0.5 M water solution of potassium hydrosulfate (KHSO4), the phase composition of the synthesized powder was presented by calcium sulfate dihydrate (gypsum, CaSO4·2H2O). When using 1 M and 2 M water solutions of potassium hydrosulfate (KHSO4), the syngenite (K2Ca(SO4)2·H2O) was found as the predominant phase in synthesized powders. According to estimations made from thermal analysis data, powders synthesized using 1.0 M and 2.0 M water solutions of potassium hydrosulfate (KHSO4) contained no more than 7.9 and 1.9 mass % of calcium sulfate dihydrate (gypsum, CaSO4·2H2O), respectively. The phase composition of products isolated from mother liquors via water evaporation consisted of syngenite (K2Ca(SO4)2·H2O) and potassium sulfate (arcanite, K2SO4). Synthesized powders can be used in preparation of biocompatible bioresorbable materials with phase compositions in the K2O-CaO-SO3-H2O system; as matrix of thermo- or photo-luminescent materials; as components reducing the setting time and increasing the strength of sulfate cements; in the fertilizing industry; and also as components of Martian regolith simulants.
The creation of new biocompatible and resorbable composite materials with an alginate matrix and fine synthetic calcium salts as a filler for potential applications in regenerative medicine is an important area of materials science. Freeze-dried porous (0.05–0.06 g/cm3) composite materials were prepared from homogeneous molding compositions containing distilled water (95 wt. %), fine inorganic powders of calcium salts (2.5 wt. %), and sodium alginate (2.5 wt. %). An aqueous solution of calcium chloride (CaCl2) and an aqueous mixed-anionic solution, which were prepared by mixing solutions of (NH4)2CO3 and (NH4)2H2P2O7 taken in different proportions, were used for syntheses of fine inorganic powders. The molar ratios (NH4)2H2P2O7)/((NH4)2CO3+(NH4)2H2P2O7) of salts used for mixed-anionic solutions preparation were established as 0 (reference powder), 0.02, 0.04, 0.08 and 0.16. Quantities of aqueous solutions of calcium chloride (CaCl2) were taken to provide a molar ratio CaCl2/((NH4)2CO3+(NH4)2H2P2O7) equal to 1.00 (reference powder), 1.02, 1.04, 1.08 and 1.16. The phase composition of synthesized inorganic powders included calcium carbonate (CaCO3) (mostly vaterite) and a quasi-amorphous phase of calcium phosphates (primarily hydrated calcium pyrophosphate (Ca2P2O7 xH2O)). All synthesized powders contained adsorbed and occluded salts present in the mother liquor after synthesis was completed, before separation of the precipitate. The mother liquors were aqueous solutions of ammonium chloride (NH4Cl) (all syntheses) and calcium chloride (CaCl2) (syntheses from mixed-anionic solutions). As components of inorganic powders used as fillers in the composite materials, ammonium chloride (NH4Cl) and calcium chloride (CaCl2) provoked a partial cross-linking of sodium alginate in the stages of preparation of molding compositions, composite samples molding, freezing, and freeze-drying. All freeze-dried porous composite materials demonstrated a high water absorption capacity of 4600–9200%. The most pronounced cross-linked effect was observed for alginate matrices loaded with powders synthesized at molar ratios CaCl2/((NH4)2CO3+(NH4)2H2P2O7) equal to 1.04 and 1.08, demonstrating the lowest water absorption and dry mass loss after dipping in distilled water for 12 h. Prepared freeze-dried porous composite materials with an alginate matrix and calcium carbonate and/or quasi-amorphous phase of calcium phosphates (primarily hydrated calcium pyrophosphate) powders, used as a filler, can be recommended for subsequent testing as an extracellular matrix for soft/hard tissue repair, as wound dressings or bone defect fillers.
Freeze-dried porous (0.05-0.06 g/cm3) composite materials were prepared from homogeneous molding compositions containing distilled water (95 wt. %), fine inorganic powders of calcium salts (2.5 wt. %) and sodium alginate (2.5 wt. %). Aqueous solution of calcium chloride (CaCl2) and aqueous mixed-anionic solution prepared by mixing solutions of (NH4)2CO3 and (NH4)2H2P2O7 taken in different proportions were used for syntheses of fine inorganic powders. Molar ratios (NH4)2Н2P2O7)/((NH4)2CO3+(NH4)2Н2P2O7) of salts used for mixed-anionic solutions preparation were established as 0 (reference powder), 0.02, 0.04, 0.08 and 0.16. Quantities of aqueous solutions of calcium chloride (CaCl2) was taken to provide molar ratio CaCl2/((NH4)2CO3+(NH4)2Н2P2O7) equal 1.00 (reference powder), 1.02, 1.04, 1.08 and 1.16. Phase composition of synthesized inorganic powders included calcium carbonate (CaCO3) (mostly vaterite) and quasi-amorphous phase of hydrated calcium pyrophosphate (Ca2P2O7 xH2O) . All synthesized powders contained adsorbed and occluded salts presented in the mother liquor after synthesis completed before separation of precipitate. Mother liquors were aqueous solutions of ammonium chloride (NH4Cl) (all syntheses) and calcium chloride (CaCl2) (syntheses from mixed-anionic solutions). As components of inorganic powders used as fillers in composite materials ammonium chloride (NH4Cl) and calcium chloride (CaCl2) provoked a partial cross-linking of sodium alginate in the stages of preparation of molding compositions, composite sample molding, freezing and freeze drying. All freeze-dried porous composite materials demonstrated high water absorption capacity 4700-9300%. The most pronounced cross-linked effect was observed for alginate matrixes loaded with powders synthesized at molar ratio CaCl2/((NH4)2CO3+(NH4)2Н2P2O7) equal 1.04 and 1.08 demonstrating lowest water absorption and dry mass-loss after dipping in distilled water for 12 hours. Prepared freeze-dried porous composite materials with alginate matrix and calcium carbonate and/or hydrated calcium pyrophosphate powders as a filler can be recommended for subsequent testing as extracellular matrix for soft/hard tissue repair, as wound dressings or bone defects fillers.