The dynamic marine atmospheric corrosion behavior of AZ31 magnesium alloy was investigated in situ exposed on the deck of marine scientific research vessel for 1 year. The marine scientific research vessel carried out five voyages from the coast of China to the western Pacific Ocean, while the navigation track and environmental data were collected and analyzed. The corrosion rate and characteristics were evaluated by using weight loss tests, scanning electron microscopy (SEM), X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), and electrochemical measurements. The corrosion rate from weight loss values was 52.23 μm∙y−1 after exposure for 1 year, which was several times higher than that of the static field exposure test in marine atmospheric environment of other reported literature. The main corrosion products were Mg5(CO3)4(OH)2·4H2O, MgCO3·3H2O and Mg2(OH)3Cl·4H2O. The corrosion was initiated from pitting corrosion and evolved into general corrosion gradually. The serious corrosion maybe due to the harsh corrosive environment with alternating changes in temperature and relative humidity caused by multiple longitude and latitude changes, and particularly high deposition rate of chloride during voyage, which was nearly twenty times that on the coast of China. This study provides effective data for the application of magnesium alloy in shipboard aircraft and other equipment, and provides a reference for indoor simulation experiments.
The effect of quenching on the corrosion resistance of Mg-7Y-1.5Nd alloy was investigated. The as-cast alloy was homogenized at 535 °C for 24 h, followed by quenching in air, water, and liquid nitrogen. Then, all of the samples were peak-aged at 225 °C for 14 h. The microstructures were studied by scanning electron microscopy, energy-dispersive spectrometry, and X-ray diffraction. Corrosion behavior was analyzed by using weight loss rate and gas collection. Electrochemical characterizations revealed that the T4-deep cryogenic sample displayed the strongest corrosion resistance among all of the samples. A new square phase was discovered in the microstructure of the T6-deep cryogenic sample; this phase was hugely responsible for the corrosion property. Cryogenic treatment significantly improved the corrosion resistance of Mg-7Y-1.5Nd alloy.
It is well known that the poor corrosion resistance of magnesium alloys is a key factor limiting their application. Field exposure is the most reliable means to evaluate the atmospheric corrosion performance of magnesium alloys. This article reviews the field exposure corrosion behavior of magnesium alloys in typical atmospheric environments (including the marine atmosphere, industrial atmosphere, etc.) in recent years. According to the literature review, it was found that there are significant regional differences in the atmospheric corrosion behavior of magnesium alloys, which is the result of the coupling of multiple factors in the atmospheric environment. By investigating the corrosion rate and corrosion products of different types of magnesium alloys in different environments, the corrosion mechanism of magnesium alloys in different environments was summarized. Specifically, environmental parameters such as atmospheric temperature, relative humidity, CO2, and chloride ion deposition rates in the marine atmospheric environment can affect the corrosion behavior of magnesium alloys. The corrosion of magnesium alloys in different industrial atmospheric environments is mainly affected by atmospheric temperature and relative humidity, as well as atmospheric pollutants (such as SO2, CO2, NO2) and dust. This review provides assistance to the development of new corrosion-resistant magnesium alloys.
Hydrogen permeation into high-strength steel during the corrosion process can deteriorate their mechanical properties, thus seriously threatening the safety of steel structures. However, the hydrogen permeation behavior of steels in corrosive marine environments is not well understood. In this study, the hydrogen permeation behavior and mechanism of AISI 4135 steel in different marine corrosion zones was investigated for the first time using an in situ hydrogen permeation monitoring system via outdoor and indoor tests. The three-month outdoor hydrogen permeation test showed that the diffusible hydrogen content of the steels exposed to the marine atmospheric, splash, tidal and immersion zone was 3.15 × 10−3, 7.00 × 10−2, 2.06 × 10−2 and 3.33 × 10−2 wt ppm, respectively. Meanwhile, results showed that the hydrogen permeation current density was positively correlated with the corrosion rate of the steel in the marine environments. This research is of great significance for guiding the safe application of high-strength steel in the marine environments.
In this work, the dynamic marine atmospheric corrosion behavior of AZ91 Mg alloy sailing from Yellow Sea to Western Pacific Ocean was studied. The corrosion rates were measured using the weight loss method. The microstructure, phase, and chemical composition of corroded samples were investigated by SEM, EDS, XRD, and XPS. The results show that the evolution of corrosion rates of AZ91 Mg alloy was divided into three stages: rapidly increasing during the first 3 months, then remaining stable for the next three months, and finally decreasing after 6 months. The annual corrosion rate of Mg alloy reached 32.50 μm/y after exposure for 12 months in a dynamic marine atmospheric environment, which was several times higher than that of the static field exposure tests. AZ91 magnesium alloy was mainly subjected to localized corrosion with more destructiveness to Mg parts, which is mainly due to the synergistic effect of high relative humidity, the high deposition rate of chloride ion, sulfur dioxide acidic gas produced by fuel combustion, and rapid temperature changes caused by the alternating changes in longitude and latitude during navigation. As the exposure time increased, the corrosion pits gradually increased and deepened. The maximum depth of the corrosion pit was 197 μm after 12 months of exposure, which is almost 6 times the average corrosion depth. This study provides scientific data support for the application of magnesium alloys in shipborne aircraft and electronic equipment. The results could provide guidance for the design of new magnesium alloys and development of anti-corrosion technologies.