The formation of defects, due to drying, in robocasted ceramic objects is an important issue arising from non-uniform shrinkage of the material during this step in the process. Common methods for shrinkage measurement are not well suited to the small size of robocasted cords or the complexity of robocasted objects. Innovative methods for shrinkage measurement were developed using non-destructive optical vision techniques with computer-controlled data acquisition, allowing measurement on millimetric cords and on specific zones of a product. The study of a single porcelain cord revealed an anisometric shrinkage related to the orientation of grains during extrusion. A differential shrinkage at the macroscopic scale was also measured on a robocasted object, indicating a moisture content gradient in the material. The methods presented in this paper are of particular relevance to real-time control of the drying process for robocasted objects.
Alumina-spinel refractory bricks, composed of 82 wt.% alumina and 18 wt.% MgAl2O4 spinel phases, are used in steel ladles due to their ability to resist chemical attack and thermal shock. Thermal shock resistance is determined, in part, by the thermal conductivity of the material. Thermal conductivity measurements for alumina-spinel refractory, three model alumina ceramics, and single crystal sapphire were made with the laser-flash technique from 20 °C to 1000 °C. At room temperature, these gave 6.5 W m−1 K−1 for the refractory, 5.8 to 22 W m−1 K−1 for the alumina ceramics, and 36 W m−1 K−1 for sapphire, despite all materials containing >81 vol.% of alumina. The differences are explained by the roles of porosity, grain boundary thermal resistance, and the spinel phase (refractory). In order to estimate the thermal conductivity of alumina grains in each material, these microstructural effects are modelled with Landauer’s relation for porosity and thermal resistors in series for grains combined with grain boundaries. For two alumina ceramics, the grains yielded similar behaviour to the single crystal. By taking the spinel phase into account with a two-phase mixture relation, the alumina grains in the refractory were estimated with a value of 31 ± 2 W m−1 K−1, close to sapphire.
Alumina-spinel refractory bricks, composed of 86 wt.% alumina phase and 13 wt.% MgAl2O4 spinel phase, are used in steel making ladles due to their ability to resist chemical attack and thermal shock. Thermal shock resistance is determined, in part, by the thermal conductivity of the material. Measurements of thermal conductivity were made with the laser flash technique from 20 °C to 1100 °C. Analysis of the influence of the microstructure on the thermal conductivity of the alumina-spinel refractory bricks was based on simplified analytical relations and validated by comparing the behaviour with four different alumina model materials. A model of thermal resistors in series was used to describe the combined effect of grains and grain boundaries on the solid phase conductivity whereas the effect of porosity was calculated with Landauer’s relation. Though the overall conductivity of the refractory brick was evaluated as 6.5 W m-1 K-1 at room temperature, the thermal conductivity of the alumina grains was deduced to be 33 W m-1 K-1, close to that of single crystal sapphire at 36 W m-1 K-1. The strongly attenuated conductivity of alumina-spinel refractory is explained by the roles of porosity, grain boundary thermal resistance and the spinel phase thermal conductivity.