Lightweight pressure vessels of type IV for hydrogen storage consist of a thermoplastic inner liner, commonly from polyethylene or polyamide. The liner is the permeation barrier against the compressed gas and must prevent the formation of cracks, also after temperature changes, for example after refueling processes. In the present work high-density polyethylene, cross-linked polyethylene, polyamide 6 and polyamide 12 were characterized by tensile tests, single notch impact tests and permeations measurements before and after a cyclic thermal aging process. The aging only lead to slight changes of mechanical properties due to post-crystallization, but to a significant decrease of permeation properties. This decrease was contributed to weakened, amorphous regions where chain splitting occurred. Considerable differences in properties resulted from different peroxide cross-linking times of polyethylene at the same temperature. A longer holding time at 200 °C led to an improvement in impact strength by a factor of more than three. However, the permeation properties decreased by about 50 %, indicating that peroxide cross-linking in the melt inhibited the formation of crystalline regions.
The decomposition of an anhydride-cured epoxy resin by subcritical hydrolysis is studied under variation of reaction temperature, decomposition duration and water volume using a batch reactor. Within the framework of a design of experiment, the process is evaluated by the gravimetric decomposition of the epoxy resin clearly showing that temperature is the most important factor. Duration and water volume have only smaller positive effects. The mass loss mechanism of the cube-shaped specimens corresponds to a heterogeneous surface degradation where material is only lost from the outer areas. The determination of glass transition temperatures after the experiments demonstrates that the water hardly affects the center of the epoxy cubes. Therefore, a core-shrinking model is successfully applied for analysis of the decomposition kinetics. The product distribution in the aqueous phase reveals a large number of organic compounds. Higher temperatures, longer durations and lower water volumes lead to an increase in decomposition product complexity and concentrations, but the degradation pathways are apparently not affected.
Polyethylene is a very common liner material for type IV pressure vessels due to its good toughness and easy processing. The property profile of the polymer can be improved by cross-linking thereby changing the nature of the polymer from thermoplastic toward more elastomeric. For this purpose, polyethylene is modified either chemically, using peroxide or silane, or physically by radiation. In the present work, a cross-linkable polyethylene grade that can be processed by rotational molding was peroxide cross-linked under variation of temperature and time. Subsequently, the material was characterized by differential scanning calorimetry, tensile tests, notched bar impact tests and permeation measurements. Two of the altogether six parameter combinations investigated did not lead to successful cross-linking resulting in very poor toughness. Stiffness, strength and permeation barrier properties, however, were much better than those of the other series due to higher crystallinity. Mechanical, physical and chemical properties changed significantly by successful cross-linking. The impact strength could be improved by a factor of more than 10. At the same time, significant losses in stiffness, strength and permeation barrier properties had to be accepted. Peroxide induced randomly distributed formation of cross-links above the melting point interfered with formation of crystalline regions upon cooling.
The influence of stitching on the delamination resistance of unidirectional glass fiber-reinforced plastic laminates depends strongly on the loading mode. The application of a lock stitch with a stitch density of 3.4 cm−1 perpendicular to the fibers results in an increase of the interlaminar fracture toughness energy, mode I, GIC by a factor of 2.7 compared to an unstitched reference laminate. The Kevlar threads are pulled out of one half of the DCB specimen leaving large frayed fiber bundles sticking out of the other half. The same stitching, however, does not improve the interlaminar fracture toughness energy, mode II, GIIC. The Kevlar threads are not able to deform the surrounding matrix thereby expending additional energy. They fail directly at the mid-plane of the ENF specimens. An increased stitch density of 11.6 cm−1 can be expected to lead to a further significant increase in the GIC value. But the tight stitching pattern causes the bonded metal hinges to tear off. The force introduction would have to be changed to enable testing of corresponding DCB and subsequently ENF specimens.
Quasi-unidirectional glass fiber non-crimp fabrics consist of a unidirectional main layer in the 0° direction stabilized by a backing layer in the 90° direction with a significantly lower amount of fibers. It is known that the backing layers impair the fatigue performance of respective reinforced plastics due to their orientation perpendicular to the main load direction. They act as damage initiators for the failure of the load-carrying unidirectional fibers. In the present work, the positive influence of the backing layers on the interlaminar fracture toughness energy – Mode I – GIC is demonstrated by tests in accordance with DIN EN 6033. The presence of backing fibers in the delamination plane can improve the GIC values by up to 43 %. Furthermore, results from evaluation according to DIN EN 6033 and ASTM D5528 are shown to have a good agreement, if the correction factor for large displacements recommended in the ASTM standard is not applied. If it is applied, however, there is a clear gap of up to 19 % between the two standards because the DIN simply does not provide a correction for large deflections.
Amine-cured epoxy resins (EP) are highly hydrophilic, particularly due to alcohol groups in the polymer network. The water absorption in humid environments leads to a reduction in the glass transition temperature (T g ) and to a deterioration in the mechanical properties. These effects have been extensively studied in the past by exposure experiments carried out at temperatures of no more than 100 °C, usually below the T g of the polymer. In this work, however, an amine-cured EP is subjected to water at 100, 150, 200 and 250 °C, all above the polymer’s T g . Thus, it is possible to achieve water absorptions of more than 10% in less than three hours. This is due to the reduced density and viscosity of the liquid phase at these temperatures, and the rubbery state of the EP. Test times can therefore be minimized compared to conventional exposure experiments in this regard. The results of dynamic mechanical analyses and tensile tests confirm the expected depression in T g (up to nearly 50 %) and decrease in tensile strength and modulus with increasing aging temperature and water absorption, respectively. This change in properties is accompanied by a light to strong yellowing of the polymer. The formation of carbonyl groups responsible for this discoloration is confirmed by infrared spectroscopy. For further application of this accelerated hydrothermal aging, however, these findings still need to be validated by comparison with conventional exposure experiments.