Particleboards with different combinations of the adhesive material imidazole, citric acid, and sorbitol were produced. Softwood sawdust from a Swedish sawmill was mixed with an aqueous solution of the chemicals and then dried to 0% moisture content prior to pressing. The boards were pressed to a target density of 700 kg m−3 at either 200 °C or 220 °C for 10 min. The hygroscopic and mechanical properties of the boards were clearly better at 220 °C than 200 °C for all used chemical combinations. A combination of imidazole (14.4 wt%) and citric acid (11.3 wt%) led to the best results, where the thickness swelling after 24 h of water immersion was 6.3% and the internal bonding strength was 0.57 MPa. The modulus of rupture and modulus of elasticity were 3.3 MPa and 1.1 GPa, respectively. Cyclic accelerated weathering showed exceptional stability with a thickness change after boiling and drying of only 2.1% compared to the initial dry thickness. This study indicates that the presence of imidazole leads to greatly improved hygroscopic properties and good internal bonding strength when used in particleboards.
The modification of Scots pine sapwood (Pinus sylvestris L.) with the heterocyclic compounds imidazole and succinimide was investigated. Pressure-impregnation with aqueous solutions containing imidazole, imidazole + citric acid, succinimide, succinimide + citric acid, and citric acid + sorbitol (CIOL®) with solid contents of 5%, 10%, and 15% was followed by oven-curing at 220 °C for 1 h. During the treatment steps, the changes in mass, bending properties, and anti-swelling efficiency (ASE) were examined. The results indicate that solid concentrations within the range of 5% to 10% were optimal. The results seem to show that there are two differing mechanisms in the modification of imidazole and succinimide, respectively. Mass loss due to heat treatment was highest in the imidazole-treated specimens, whereas it remained low and concentration-independent in the succinimide-treated specimens. After three cycles, the ASE reached 31% for the imidazole-treated specimens and improved to 38% with the addition of citric acid. For succinimide, the ASE increased from 17% to 41%. The bending properties generally showed improvement, except for succinimide + citric acid and CIOL®, which displayed a reduced modulus of rupture. Chemical analyses are warranted to fully understand the reaction mechanisms of these treatments. The positive effects of imidazole treatment are suggested to stem from a thermal reaction between the chemical and the wood, indicated by substantial mass loss during leaching and specimen darkening. Succinimide and citric acid might exhibit polymerization with each other and with wood components, which is akin to the CIOL® process. Further research should delve into the reaction mechanisms and the impact of imidazole and succinimide on biological durability.
Modification of Scots pine sapwood (Pinus sylvestris L.) with heterocyclic compounds, imidazole and succinimide, was investigated. Pressure-impregnation with aqueous solutions containing imidazole, imidazole + citric acid, succinimide, succinimide + citric acid, and citric acid + sorbitol (CIOL®) at 5%, 10%, and 15% solid content was followed by oven-curing at 220 °C for 1 hour. Mass changes during treatment steps, bending properties, and anti-swelling efficiency (ASE) were examined. Results indicate that solid concentrations within the range of 5% to 10% were optimal. Results seem to show there are two differing mechanisms in the modification of imidazole and succinimide, respectively. Mass loss due to the heat treatment was highest in imidazole-treated specimens, whereas it remained low and concentration-independent in succinimide-treated specimens. ASE after three cycles reached 31% for imidazole-treated specimens and improved to 38% with the addition of citric acid. For succinimide, ASE increased from 17% to 41%. Bending properties generally showed improvement, except for succinimide + citric acid and CIOL®, which displayed a reduced modulus of rupture. Chemical analyses are warranted to fully understand the reaction mechanisms of the treatments. Imidazole treatment's positive effects are suggested to stem from a thermal reaction between the chemical and wood, indicated by substantial mass loss during leaching and specimen darkening. Succinimide and citric acid might exhibit polymerization with each other and wood components, akin to the CIOL® process. Further research should delve into reaction mechanisms and the impact of imidazole and succinimide on biological durability.