Chitosan (CS) and its derivatives show antimicrobial properties. This is of interest in preventing and treating denture stomatitis, which can be caused by fungi. Therefore, the aim of this study was the development of a novel antifungal denture base material by modifying polymethyl methacrylate (PMMA) with CS-salt and characterizing its antifungal and surface properties in vitro. For this purpose, the antifungal effect of chitosan-hydrochloride (CS-HCl) or chitosan-glutamate (CS-G) as solutions in different concentrations was determined. To obtain modified PMMA resin specimens, the CS-salts were added to the PMMA before polymerization. The roughness of these specimens was measured by contact profilometry. For the evaluation of the antifungal properties of the CS-salt modified resins, a C. albicans biofilm assay on the specimens was performed. As solutions, both the CS-G and CS-HCl-salt had an antifungal effect and inhibited C. albicans growth in a dose-dependent manner. In contrast, CS-salt modified PMMA resins showed no significant reduced C. albicans biofilm formation. Furthermore, the addition of CS-salts to PMMA significantly increased the surface roughness of the specimens. This study shows that despite the antifungal effect of CS-salts in solution, a modification of PMMA resin with these CS-salts does not improve the antifungal properties of PMMA denture base material.
In oral sciences, chitosan application is of interest due to its antimicrobial and hemostatic activity. Chitosan coating of dentures and other intraoral devices could be beneficial for treatment of denture stomatitis or in the management of postoperative bleeding. Disinfection of dentures and prosthodontic materials is crucial before their use in patients. This study investigated the influence of chemical disinfectants on chitosan-coated surfaces. A total of 100 specimens were made: 50 of PMMA (polymethyl methacrylate), and 50 of PETG (polyethylene terephthalate glycol-modified) material and coated with 2% chitosan acetate solution. In each material, 5 groups (10 specimens each) were established and disinfected with Printosept-ID (L1), MD 520 (L2), Silosept (L3), or Dentavon (L4), or stored in distilled water (L0, control group). After disinfection, all specimens underwent abrasion tests (30,000 cycles in a tooth-brushing simulator). Areas without chitosan coating were measured by digital planimetry both before and after the disinfection/abrasion procedure and a damage-score was calculated. Regarding chitosan coating, the statistical analysis showed a significant influence of the disinfectants tested and significant differences between disinfectants (p < 0.05). Chitosan coating was most stable on PMMA and PETG after disinfection with MD 520 (L2). Otherwise, active oxygen containing disinfectants (L3, L4) led to the greatest alterations in the chitosan coating.
Chitosan (CS) and its derivatives show antibacterial and antifungal properties and could help treat and prevent denture stomatitis (DS). Mechanical and surface properties of resilient denture liners were evaluated when modified with CS salts. CS-hydrochloride (CS-HCl) and CS-glutamate (CS-G) were added to resilient denture liners Ufi Gel P and Coe-Soft at four different concentrations (0.1%, 0.2%, 0.4%, 1% w/w) from which specimens were produced, as well as a control group of each material with no added CS salt. Ten specimens per group (Ø 35 mm, height 6 mm) were manufactured. They were stored in distilled water at 37 °C for a total of 30 days (d). Shore A hardness (SHA) and surface roughness (Ra) were evaluated after 24 h (T1), 7 d (T2), 14 d (T3) and 30 d (T4). Kruskal–Wallis and U-test (Bonferroni-Holm adjusted) were used for statistical analysis (p ≤ 0.05). Ra increased significantly once CS salts were added. SHA increased significantly for some groups, but all specimens fulfilled requirements set by ISO 10139-2:2016. Modification with CS salts does not influence the mechanical properties of the modified resilient denture liners in a clinically relevant manner. Despite the increased roughness, the concept is suitable for further studies. Especially antimicrobial/antibiofilm studies are needed.
Chitosan is a cationic natural polymer that is widely used as a topical dressing in wound management. Temporary coatings of removable denture bases with chitosan might be useful as supportive treatment in oral medicine. The aim of this study was to analyze the thickness, uniformity, and adhesive strength of chitosan coatings on simulated denture bases made from polymethyl methacrylate (PMMA). According to a standardized protocol, 20 PMMA cylinders (13 mm diameter, 5 mm in height) as well as 20 cubes (a = 25 mm) with intaglio U-shaped profiles were manufactured to simulate average sized alveolar ridges. Cylinders as well as cubes were divided into four test series with n = 5 each. After sandblasting with silica-modified alumina, one frontal surface of the PMMA cylinders and the intaglio surfaces of the U-shaped profiles was coated with chitosan acetate solution according to the following protocols: one layer of 2% chitosan acetate solution (test series I), one layer of 4% chitosan acetate solution (test series II), two layers of 2% chitosan acetate solution (test series III), and two layers of 4% chitosan acetate solution (test series IV). After drying and neutralization with NaOH, each cube was cut transversely and the coating thickness across the U-shaped profile assessed with a light microscope. Adhesive strength was evaluated by simulated tooth brushing and the loss of chitosan coating was evaluated qualitatively. Statistical analysis used Friedman ANOVA test for dependent samples and Kruskal-Wallis test for independent samples, post-hoc Dunn’s test (p < 0.05), and binomial test (p = 0.05). The mean chitosan coating thicknesses in the depth of the U-profiles were 71 µm (test series I), 77 µm (test series II), 121 µm (test series III), and 517 µm (test series VI). The thickness continuously decreased with rising angulation of the U-profile side walls. In test series I, the chitosan coating thickness significantly dropped above a 30° angulation of the U-profile side walls. In test series II to IV, the chitosan thickness drop was not statistically significant at angulations of 30° and 60°, but was at 90° angulation of the U-profile side walls. Adhesion strength was rated fair to good and did not differ significantly among the four test series. The coating technique described revealed chitosan layers with overall good adhesion strength but differing thicknesses. Coatings with one or two layers of 4% chitosan acetate solution allowed a relatively uniform chitosan thickness and thus might be usable in oral medicine.