This report documents work performed under the Spent Fuel and Waste Disposition for the US Department of Energy (DOE) Office of Nuclear Energy (NE) Spent Fuel and Waste Science and Technology program. This work was performed to fulfill the Level 2 Milestone M2SF-17OR010201021, “Documentation of Non-destructive Tests on Sister Pins,” within work package SF-17OR01020102. The High Burnup Spent Fuel Data Project, sponsored by DOE-NE, is focused on understanding the effects of long-term storage and transportation on high burnup (HBU) (>45 gigawatt days per metric ton uranium) light water reactor fuel. The goals of the project are to “provide confirmatory data for model validation and potential improvement, provide input to future spent nuclear fuel (SNF) dry storage cask design, support license renewals and new licenses for Independent Spent Fuel Storage Installations (ISFSIs), and support transportation licensing for high burnup SNF". In support of project goals, 25 sister rods were removed from fuel assemblies at the North Anna Power Station. Nine rods were removed from the project assemblies, and 16 rods were removed from similar HBU assemblies. The 25 sister rods were shipped to Oak Ridge National Laboratory (ORNL) Irradiated Fuels Examination Laboratory (IFEL) in early 2016 for detailed nondestructive examination (NDE)more » and destructive examination (DE). The detailed examinations will provide essential information on the physical state of the HBU rods and the fuel contained in the rods prior to loading, drying, and long-term dry storage. Similar tests will be performed at the end of the long-term storage period to identify any changes in the fuel rods’ properties during the dry storage period. « less
The High Burnup Spent Fuel Data Project, sponsored by the U.S. Department of Energy Office of Nuclear Energy, is focused on understanding the effects of long-term storage and transportation on high burnup (HBU) (>45 GW days per tonne uranium) light water reactor fuel. The project includes 32 HBU spent nuclear fuel (SNF) assemblies (the project assemblies) that are stored in a typical independent spent fuel storage installation (ISFSI) and 25 “sister rods”—9 SNF rods that were removed from the fuel assemblies prior to insertion to the ISFSI and 16 SNF rods removed from similar HBU assemblies. The sister rods provide a baseline of the condition of the HBU rods before loading, drying, and long-term dry storage. The project assemblies will be inspected after 10 years, and the physical state of the stored rods will be compared with the condition of the sister rods to identify any changes in physical properties during the dry storage period. This work focuses on key results from the nondestructive postirradiation examinations of the sister rods and summarizes the results of detailed visual examinations, gamma scans, dimensional measurements, and eddy current liftoff measurements of the combined Chalk River unidentified deposits and oxide layer on the waterside surface of the rod. The data are used to calculate fuel rod and pellet stack growth rates, estimated remaining fuel rod plenum volumes, and the percentage change in fuel rod cladding diameter.
At present, spent nuclear fuel (SNF) assemblies discharged from US commercial power plants are placed into dry storage following a short cooling time (45 GWd/MTU) SNF rods to address knowledge and data gaps related to extended interim storage and eventual transportation for disposal. The rods examined include four different kinds of fuel rod cladding: standard Zircaloy-4 (Zirc-4), low-tin (LT) Zirc-4, ZIRLO, and M5. Three rods were subjected to a thermal transient to assess the effects of decay-heat-driven high temperatures expected during vacuum drying of the fuel as it is prepared for interim dry storage. The examinations focus on the composite fuel rod performance, as compared with the performance of defueled rod cladding, and establish the baseline mechanical properties of a fuel rod before interim dry storage. The key results of these examinations are presented, including the measured mechanical and fatigue properties, observations of cladding hydrogen pickup and hydride reorientation effects on rod performance, effects of the simulated drying temperatures on rod performance, and general conclusions of SNF performance in extended interim dry storage and transport. The rods were found to be strong and durable in the expected loading conditions, even considering the formation of radial hydrides associated with vacuum drying. The combined testing provides a broad body of data supporting extended interim storage and transportation performance of HBU spent fuel.