In this study, the purpose was to improve outdoor performance of cement bonded wood composite due to their biodegradation and sensitivity to moisture especially in warm and humid climates. Cement bonded wood composites were treated with different concentrations (10 %, 25 %, 50 %, 75 % and 100 %) of water repellent. Water repellent used was an organo-silicon based, nano-sized, eco-friendly, water-based agents. Dipping and pressure systems were applied for composite treatment. Water absorption, thickness swelling, accelerated weathering, color changes and mechanical properties after accelerated weathering were determined for treated and untreated cement-bonded composites. Results showed that treatment of composites with water repellent provided a transparent layer on composite surface. Thus, lower water absorption and thickness swelling results in the beginning of immersion in water. Treated and untreated composites were exposed to an accelerated weathering test for 350 h. Their mechanical strength including modulus of rupture, modulus of elasticity and internal bonding properties were decreased after 350 h of weathering. However, overall results after weathering test showed that all panels’ mechanical properties provided minimum modulus of rupture, modulus of elasticity and internal bonding requirements of the EN standards.
26 July 2017 in High Temperature Materials and Processes
In this study, the effects of hardener type (ammonium chloride and ammonium nitrate) and board thickness on the physical (density, thickness swelling and water absorption), mechanical (modulus of rupture, modulus of elasticity, internal bond strength, screw withdrawal resistance and surface durability) and formaldehyde content of particleboard were investigated. Three types panels were produced using 11-9% urea-formaldehyde adhesive (core and surface, respectively), with 650kg/m3 target density, 150°C pressing temperature, 20-24kg/cm2 pressure, and 6min of pressing time. The analyses revealed that use of ammonium nitrate for particleboard manufacturing resulted in improved water absorption and thickness swelling properties after 24h of immersion in water. In addition, the using ammonium nitrate has no significant effect by Modulus of rupture (MOR) and modulus of elasticity (MOE). However, internal bond strength, screw withdrawal resistance and surface durability properties were positively affected by using ammonium nitrate. Formaldehyde content value was decreased by about 5%. The study demonstrated that the boards made of ammonium nitrate meet the requirements for general standard and building materials
31 December 2019 in Journal of Anatolian Environmental and Animal Sciences
In this study, it is aimed to determine the effect of the use of different types cement and accelerator on the physico-mechanical properties of cement-bonded particleboards. Within this scope, two types of cements (calcium aluminate cement and Super white CEM I 52.5 R) and accelerators (aluminum sulfate and calcium chloride) were used in the production of boards. Therefore, CBPBs with 1200 kg/m3 target density and 1/2.75 wood-cement ratio were produced. Based on cement weight 1.5% accelerators were used. The test results obtained were evaluated according to EN 634-2 (2009). According to result, density values of the boards were changed with using depending on cement and accelerator types. The use of super white cement and calcium chloride positively affected the both mechanical properties and dimensional stability of the boards. The use of calcium aluminate cement and aluminum sulfate resulted in lower strength properties.
16 December 2016 in Mugla Journal of Science and Technology
Bu çalışmada fıstık çamı (Pinus Pinea L.) yongaları ve kozalak atıklarıyla üretilen 3 tabakalı yongalevhaların bazı teknolojik özellikleri araştırılmıştır. Çam Yongası ve kozalak karışım oranına göre 4 adet levha tipi üretilmiştir (%100/0, %50/50, %0/100 ve %40/60). Yongalevhaların Dış/orta tabaka kullanım oranı %40:60’dır. 400×400×12 mm boyutlarında üretilen levhaların özgül ağırlığı 700 g/cm 3 olup, pres basıncı 24-26 kPa/cm 2 ’dir. Üretim sonucunda levhaların Limit oksijen indeksi (LOI) değerleri (ASTM D 2863), çürüklük dayanımı (EN 113) ve yüzey pürüzlülükleri(DIN 4768) belirlenmiştir. Yapılan çalışma sonucunda atık çam kozalağı kullanımının yonga levhaların özelliklerini etkilediği belirlenmiştir. Kozalak kullanım oranının artmasıyla çürüklük dayanımı artmıştır. Fakat LOI ve yüzey pürüzlülüğü değerleri de karışımdaki kozalak kullanım oranının artması ile artış göstermiştir.