Samples of U75V steel with different contents of lanthanum (La) and cerium (Ce) were melted using a vacuum induction furnace, then were rolled and forged. The morphology, number, aspect ratio, type, and impact properties of the inclusions were tested and analysed. The results indicate that in the absence of rare earth, there are Al2O3–CaO–SiO2–MnO, MnS–Al2O3–CaO–SiO2 composite inclusions, and MnS in U75V steel. After adding a mixture of rare earth elements La–Ce to the steel, the inclusions transform into (La–Ce)2O2S, (La–Ce)S, Ce2O3, (La–Ce)2O2S–(La–Ce)S, and (La–Ce)2O2S–CaO composite inclusions. Adding a mixture of rare earth (La–Ce) significantly reduces the quantity, size, and aspect ratio of the inclusions. The distinction resides in the varying ratio of lanthanum to cerium, resulting in dissimilar circumstances. After adding rare earth lanthanum and cerium, the proportion of small–sized inclusions increases. Sample 2 has the highest proportion of small–sized inclusions. Impact tests and grain size analysed were conducted during the experiment. It was found that sample 2 has the smallest grains and the best impact performance. The “Nailing force” of rare earth inclusions on the microstructure of the steel samples was calculated, and the results show that the addition of rare earth to the steel reduces the microstructural grain size due to the “Nailing force” of the rare earth inclusions. The microstructural grain size of the steel is different due to the differences in the rare earth inclusions generated by different rare earth contents, and this is the fundamental reason for the different microstructural grain sizes of the steel after adding rare earth.
To investigate the effects of multiple-element rare earth addition on U75V steel, this study produced three types of steel: sample 1 steel without rare earths, sample 2 steel containing 0.0035% La and 0.018% Ce, and sample 3 steel containing 0.02% La and 0.0023% Ce. Microstructural analysis showed that the addition of rare earth elements modified the MnS and silicoaluminate inclusions into RE2O2S and RE2O2S–oxide complexes, which reduced the number and size of inclusions while simultaneously refining the microstructure, including the grain size and the spacing of pearlite layers. Concurrently, RE addition enhanced the steel’s mechanical properties, with the degree of enhancement dependent on RE content; sample 2 exhibited the most balanced improvement. Compared to sample 1, the hardness of samples 2 and 3 increased by 15.3% and 3.6%, respectively, and their tensile strength increased by 7.9% and 6.8%, respectively. Meanwhile, their coefficients of friction decreased significantly, by 69.5% and 22.1%. The impact toughness was also enhanced by RE addition, with both samples 2 and 3 showing higher values than sample 1 at room temperature and moderate low temperatures. Nevertheless, a distinct reversal was observed at −60 °C, where the impact energy of sample 3 was 23.5% lower than that of sample 2. This result implies that while moderate RE addition is beneficial, an excessive amount can adversely affect the toughness under cryogenic conditions.
Slag entrainment within the mold is a significant cause of surface defects in continuously cast slabs. As a key component for controlling molten steel flow, the structure of the submerged entry nozzle directly influences the flow field characteristics and slag entrainment behavior within the mold. This paper employs a 1:4-scale water–oil physical model combined with numerical simulation to investigate the effects of elliptical and circular submerged entry nozzles on slag entrainment behavior in a wide slab mold under different casting speeds and immersion depths. High-speed cameras were used to visualize meniscus fluctuations and oil droplet entrainment processes. An alternating control variable method was employed to quantitatively delineate a slag-free “safe zone” and a “slag entrainment zone” where oil droplets fall, determining the critical casting speed and critical immersion depth under different operating conditions. The results show that, given the nozzle immersion depth and slag viscosity, the maximum permissible casting speed range without slag entrainment can be obtained, providing a reference for industrial production parameter control. The root mean square (RMS) of surface fluctuations was introduced to characterize the activity of the meniscus flow. It was found that the RMS value decreases with increasing nozzle immersion depth and increases with increasing casting speed, showing a good correlation with the frequency of slag entrainment. Numerical simulation results show that compared with elliptical nozzles, circular nozzles form a more symmetrical flow field structure in the upper recirculation zone, with a left–right vortex center deviation of less than 5%, resulting in higher flow stability near the meniscus and thus reducing the risk of slag entrainment.