A 5.0-at.% Nd-doped La0.64Gd0.41Sc2.95(BO3)4 (Nd:LGSB) borate laser crystal was successfully grown by the Czochralski method, for the first time to our knowledge. The spectroscopic properties of the grown crystal are discussed and 1 µm laser emission, under end-pumping with a fiber-coupled diode laser at 807 nm, is reported. A c-cut Nd:LGSB medium yielded 1.35 W continuous-wave output power at 0.63 overall optical-to-optical efficiency, with respect to the absorbed pump power, together with the high 0.68 slope efficiency. With an a-cut Nd:LGSB sample, 0.81 W output power at 0.52 optical-to-optical efficiency was obtained. The laser emission performances under quasi-continuous wave pumping are presented as well, for both c-cut and a-cut crystals. Passive Q-switching was investigated with a semiconductor saturable absorber mirror (SESAM). Laser pulses with 2.2 µJ energy and 32.8 ns durations were recorded from a-cut Nd:LGSB. The average output power reached 0.36 W at 1.55 W absorbed pump power. Passive mode-locking with SESAM was achieved in a long Z-type resonator. Ultrashort pulses with 0.19 W average power, 1.63 nJ energy, and 1.43 ps pulse duration, at 118 MHz repetition rate, are demonstrated for the a-cut Nd:LGSB medium.
Spectroscopic characteristics of RE3+ ions (RE = Sm, Dy, and Pr) doped in partially disordered Ca3Nb1.6875Ga3.1875O12-CNGG and Ca3Li0.275Nb1.775Ga2.95O12-CLNGG crystals are reviewed in detail to assess their prospects as laser crystals with emission in the visible spectral domain. All investigated crystals were grown using the Czochralski crystal growth technique. High-resolution absorption and emission measurements at different temperatures, as well as emission dynamics measurements, were performed on the grown crystals. The spectroscopic and laser emission characteristics of the obtained crystals were determined based on the Judd-Ofelt parameters. The obtained results indicate that CNGG:RE3+ and CLNGG:RE3+ (RE = Sm, Dy, and Pr) crystals can be promising materials for lasers in the visible range.
Herein we present a roadmap for tailoring the crystal growth conditions, near-infrared (NIR) laser emission, and self-frequency doubling (SFD) performances of newly developed Nd-doped LaxGdySc4−x−y(BO3)4 (Nd:LGSB) crystals. Three different Nd3+ doping concentrations of 2.3 at.%, 3.5 at.%, and 4.6 at.% were investigated. Considering their incongruent melting, special conditions were employed for the growth using the Czochralski technique. Laser emission performances at 1062 nm in the CW regime were evaluated for uncoated crystal samples with different orientations (a-cut, c-cut, and SFD-cut). The highest slope efficiency ηsa = 0.68 was obtained for the 4.6 at.% c-cut Nd:LGSB crystal, with a randomly polarized emission. The a-cut 4.6 at.% Nd:LGSB crystal delivered a linearly polarized beam with a slope efficiency ηsa = 0.63. The SFD-cut 2.3 at.% and 3.5 at.% Nd:LGSB crystals achieved slightly lower efficiencies of ~ 0.56. The SFD capabilities of 2.3 at.% and 3.5 at.% Nd:LGSB crystals were also explored. Green laser emission at ~531 nm was achieved with a diode-to-green conversion efficiency increasing significantly from 0.17% to 1.44%, respectively. These results demonstrate that the Nd-doping concentration, crystal orientation, and sample length of Nd:LGSB crystals, must be carefully selected depending on the specific requirements of the intended application.
Buried depressed-cladding waveguides were fabricated in 0.7-at.% Nd:Ca3Li0.275Nb1.775Ga2.95O12 (Nd:CLNGG) and 7.28-at.% Yb:CLNGG disordered laser crystals grown by Czochralski method. Circular waveguides with 100 μm diameters were inscribed in both crystals with picosecond (ps) laser pulses at 532 nm of 0.15 μJ energy at 500 kHz repetition rate. A line-by-line writing technique at 1 mm/s scanning speed was used. Laser emission at 1.06 μm (with 0.35 mJ pulse energy) and at 1.03 μm (with 0.16 mJ pulse energy) was obtained from the waveguide inscribed in Nd:CLNGG and Yb:CLNGG, respectively, employing quasi-continuous wave pumping with fiber-coupled diode lasers. The waveguide realized in RE3+-doped CLNGG crystals using ps-laser pulses at high repetition rates could provide Q-switched or mode-locked miniaturized lasers for a large number of photonic applications.
This paper reviews the progress in developing the LaxYySc4-x-y(BO3)4-LYSB and Yb-doped LaxYySc4-x-y(BO3)4-LYSB:Yb huntite-type crystals grown by the Czochralski method as new candidates for the next generation of nonlinear optical (NLO) and/or laser crystals. Considering the incongruent melting of these crystals, the initial compositions of the melt and the pulling and rotation rates were optimized. Additionally, a special thermal setup was engineered to grow LYSB-type crystals by the Czochralski crystal growth method. The chemical compositions of the LYSB and LYSB:Yb grown crystals were found to be La0.78Y0.32Sc2.90(BO3)4 and La0.78Y0.32Yb0.04Sc2.86(BO3)4, respectively. Therefore, for the LYSB:Yb crystal, the doping concentration of Yb3+ ions was considered to be 4 at.% with respect to the nonstoichiometric (La1-xYx)1.25Sc2.75(BO3)4 undoped compounds, i.e., LYSB:Yb (4 at.%). In terms of NLO properties, the obtained results demonstrate that LYSB and LYSB:Yb (4 at.%) crystals possess remarkable properties specific to huntite-type crystals. The main advantage of these crystals consists in the fact that they may be obtained with large dimensions and excellent optical quality by the Czochralski method, which recommends them as a new class of highly efficient crystals for different NLO applications, including second harmonic generation (SHG) of high-power or high-energy laser beams. The laser performances of the LYSB:Yb (4 at.%) crystal prove its favorable intrinsic properties to generate laser emissions in the 1 µm range with high efficiency. The efficient laser emission at ~1028 nm together with good NLO characteristics to convert its own emission into emission at ~514 nm via SHG make the LYSB:Yb (4 at.%) crystal a very promising active medium to be used in self-frequency doubling configuration.