Cermet coatings deposited using high-velocity oxy-fuel (HVOF) are widely used due to their excellent wear and corrosion resistance. The new agglomeration–rapid sintering method is an excellent candidate for the preparation of WC–Co–Cr feedstock powders. In this study, four different WC–10Co–4Cr feedstock powders containing WC particles of different sizes were prepared by the new agglomeration–rapid sintering method and deposited on steel substrates using the HVOF technique. The microstructures and mechanical properties of the coatings were investigated using scanning electron microscopy, X-ray diffraction, nanoindentation, and Vickers indentation. The through-thickness residual stress profiles of the coatings and substrate materials were determined using neutron diffraction. We found that the microstructures and mechanical properties of the coatings were strongly dependent on the WC particle size. Decarburization and anisotropic mechanical behaviors were exhibited in the coatings, especially in the nanostructured coating. The coatings containing nano- and medium-sized WC particles were dense and uniform, with a high Young’s modulus and hardness and the highest fracture toughness among the four coatings. As the WC particle size increased, the compressive stress in the coating increased considerably. Knowledge of these relationships enables the optimization of feedstock powder design to achieve superior mechanical performance of coatings in the future.
Owing to the increasing demand for tribological brakes for space applications, the development of novel materials and advanced technologies is necessary. This paper presents the design, characterization, and realization of powder metallurgy processed metal-matrix friction materials intended for the above-mentioned tribological brakes. Selecting appropriate ingredients, which provides an effective way to tailor the properties of the friction material, is evolving as a strategy to meet the design requirements. The tribological behaviors of the friction material are experimentally investigated under different conditions, and special attention is focused on the vacuum tribology. Examinations and analyses of the friction surface and subsurface corroborate the wear mechanism. In addition, the erosion resistances of the friction material are evaluated by exposure tests of ultraviolet irradiation and atomic oxygen. Finally, present and potential space applications of the friction material are also introduced based on experimental studies.
In the present work, the mechanical and tribological properties of carbon nanotube (CNT)-reinforced Cu matrix composites featuring 0–1.8 vol% CNTs prepared by spark plasma sintering under dry sliding and boundary lubrication conditions were investigated. The results of microstructure revealed that the bonding interface in Cu/CNT composites was very well established. Additionally, the addition of CNTs has a positive effect on improving the hardness and tensile strength of the composites, while the stress–strain response quasi-static tensile test confirms the same results. CNTs are proved to lead to certain self-lubrication. The addition of CNTs could result in decreased coefficient of friction (COF) and wear rates by reducing adhesive wear under dry sliding conditions, while the oil lubricating film was the major reason for decreased COF under boundary lubrication conditions.
A series of Al2O3–Al2TiO5 ceramic composites with different Al2TiO5 contents (10 and 40 vol.%) fabricated at different sintering temperatures (1450 and 1550 °C) was studied in the present work. The microstructure, crystallite structure, and through-thickness residual stress of these composites were investigated by scanning electron microscopy, X-ray diffraction, time-of-flight neutron diffraction, and Rietveld analysis. Lattice parameter variations and individual peak shifts were analyzed to calculate the mean phase stresses in the Al2O3 matrix and Al2TiO5 particulates as well as the peak-specific residual stresses for different hkl reflections of each phase. The results showed that the microstructure of the composites was affected by the Al2TiO5 content and sintering temperature. Moreover, as the Al2TiO5 grain size increased, microcracking occurred, resulting in decreased flexure strength. The sintering temperatures at 1450 and 1550 °C ensured the complete formation of Al2TiO5 during the reaction sintering and the subsequent cooling of Al2O3–Al2TiO5 composites. Some decomposition of AT occurred at the sintering temperature of 1550 °C. The mean phase residual stresses in Al2TiO5 particulates are tensile, and those in the Al2O3 matrix are compressive, with virtually flat through-thickness residual stress profiles in bulk samples. Owing to the thermal expansion anisotropy in the individual phase, the sign and magnitude of peak-specific residual stress values highly depend on individual hkl reflection. Both mean phase and peak-specific residual stresses were found to be dependent on the Al2TiO5 content and sintering temperature of Al2O3–Al2TiO5 composites, since the different developed microstructures can produce stress-relief microcracks. The present work is beneficial for developing Al2O3–Al2TiO5 composites with controlled microstructure and residual stress, which are crucial for achieving the desired thermal and mechanical properties.