Saprolitic nickel laterite is characterized by relatively low iron and nickel contents. Iron and nickel oxides are reduced to form fine ferronickel particles that disperse and embed in silicates in the reduction process, limiting the application of magnetic separation to extract ferronickel. Additives are applied to promote the aggregation and growth of ferronickel particles, then the large ferronickel particles will be separated by fine grinding and recovered via magnetic separation. Calcium sulphate is considered to be capable of increasing the size of ferronickel particles considerably. Due to the decomposition of calcium sulphate in the reduction process, the mechanism of calcium sulphate on the aggregation and growth of ferronickel particles should be conducted studied in-depth. The current work explores the effects of calcium sulphate, elemental sulphur, and calcium oxide on the formation of ferronickel particles in a saprolitic nickel laterite ore. The results showed that the formation of an Fe-FeS eutectic and the mineral structure transformation contributed by calcium oxide were all conducive to the mass transfer of ferronickel particles in gangue, ferronickel particles aggregated and grew up at the boundary between the hole and the gangue. The self-reduction, fine grinding, and magnetic separation of nickel laterite ore in the presence of three types of additive were examined. Nickel laterite ore with 7.88 wt% coal, 12 wt% calcium sulphate reduced at 1200 °C for 30 min, a ferronickel concentrate of Ni 8.08 wt%, and Fe 79.98 wt% was obtained at a nickel and iron recovery of 92.6% and 79.9%, respectively.
Owing to the superior reduction kinetics of limonite and goethite relative to silicates, coupled with the poor beneficiation performance of saprolite-type laterite, the direct carbothermal reduction of saprolite-type laterite exhibits limited nickel selectivity. This study leverages the selective oxidation effect of CO-CO2 atmosphere on metallic iron and its suppression of Fe2+ reduction to promote iron migration from oxides into the silicate phase, achieving homogenization and thereby negating its kinetic advantage in reduction. Parameter optimization experiments revealed that treating pre-reduced minerals with a 30 vol% CO atmosphere at 1200 °C for 20 minutes achieves complete iron homogenization within the silicate phase. Compared with the nickel-iron alloy (containing less than 10 wt% Ni) obtained via RKEF process, the combination of pre-reduction, CO-CO2 treatment, and melting reduction process yielded nickel-iron alloys with nickel contents of 52.1 wt% (FeNi50 alloy) and 64.2 wt% at carbon consumptions of 4.0 wt% and 3.83 wt%, respectively, accompanied by nickel recovery rates of 95.5% and 91.2%. Furthermore, the enrichment of Fe2+ in the slag significantly reduces its melting point to approximately 1450 °C, enabling complete slag-metal separation after smelting at 1550 °C for 10 minutes.
Owing to the superior reduction kinetics of limonite and goethite relative to silicates, coupled with the poor beneficiation performance of saprolite-type laterite, the direct carbothermal reduction of saprolite-type laterite exhibits limited nickel selectivity. This study leverages the selective oxidation effect of CO-CO2 atmosphere on the metallic iron of pre-reduced minerals, as well as its suppression of Fe2+ reduction, to promote iron migration from oxides to the silicate phase, achieving homogenization and thereby negating its kinetic advantage in reduction. Parameter optimization experiments revealed that treating pre-reduced minerals with a 30 vol% CO atmosphere at 1200 °C for 20 min achieves complete iron homogenization within the silicate phase. Compared with the nickel–iron alloy (containing less than 10 wt% Ni) obtained via the RKEF process, the combination of pre-reduction, CO-CO2 treatment, and the melting reduction process yielded nickel–iron alloys with nickel contents of 52.1 wt% (FeNi50 alloy) and 64.2 wt% at carbon consumptions of 4.0 wt% and 3.83 wt%, respectively, accompanied by nickel recovery rates of 95.5% and 91.2%. Furthermore, the enrichment of Fe2+ in the slag significantly reduces its melting point to approximately 1450 °C, enabling complete slag–metal separation after smelting at 1550 °C for 10 min.