We report the first fabrication of sputtered carbon, solid-phase microextraction (SPME) fibers. These fibers have competitive extraction capabilities compared with the commercial carbon wide range (CWR) SPME fiber. This report also includes a demonstration of a newly developed SPME test mix that includes 15 different compounds with a wide range of functional groups and chemical properties. The fiber fabrication process involves sputtering carbon onto fused silica fibers, and the effects of throw distance on the morphology of the carbon coatings were studied. Four different carbon coating thicknesses were evaluated, with PDMS added as a stationary phase. These fibers were characterized with multiple analytical techniques, including scanning electron microscopy (SEM), X-ray photoelectron spectroscopy (XPS), water contact angle (WCA) goniometry, as well as headspace (HS) and direct immersion (DI)–SPME–GC–MS. The best (11.5 µm) sputtered carbon SPME fibers, with and without PDMS, were evaluated using the new evaluation mix and compared with the commercial CWR fiber and a previously sputtered/developed silicon fiber. The new probe mix helped elucidate differences among the fibers, which would have been missed by current commercial test mixes. The sputtered carbon SPME fibers showed similar functional group selectivity as commercial CWR fibers. However, the sputtered carbon fibers showed higher responses per volume compared with the commercial CWR fiber, indicating the porous morphology of the sputtered carbon has the ability to overcome large phase thickness/volume discrepancies and increase the relative recovery for various compounds.
We report the optical functions of diphenylsiloxane-dimethylsiloxane (DPS-DMS) copolymer as determined from reflection spectroscopic ellipsometry (SE) and transmission ultraviolet-visible data, which were generated over 191–1688 nm from a commercial sample of DPS-DMS. This material is a random, linear copolymer terminated with silanol groups that is a liquid at room temperature and pressure. Both reflection and transmission measurements required special experimental considerations. The reflection SE measurements utilized the “rough-surface” method, wherein the liquid was poured onto a roughened (frosted) glass slide, which scatters the reflected light leaving only the reflection from the liquid surface. That is, there is effectively no substrate or material beneath the liquid that affects the ellipsometry measurements or that needs to be modeled. Transmission measurements were obtained via a dual cuvette approach to eliminate the effects of the cuvettes. The reflection data provided the refractive index across the entire spectral range as well as the extinction coefficient at ultraviolet wavelengths. The transmission measurements provided input for the extinction coefficients at visible and near infrared wavelengths, where the liquid is transparent or semitransparent. The reflected SE data were modeled using a Sellmeier dispersion model and six Gaussian oscillators plus a surface roughness layer. This produced a good fit with a mean squared error (MSE) of 2.41. For example, we obtained the following n(λ) values, where λ is the wavelength in nanometers: n(300) = 1.534, n(500) = 1.477, and n(1000) = 1.458. As expected, the refractive index of DPS-DMS is higher than that of liquid polydimethylsiloxane.
Amorphous carbon nanotubes (aCNTs) were synthesized by AAO (anodic aluminum oxide) template at a temperature 500 °C in nitrogen atmosphere using the citric acid as a carbon source without the help of any catalyst particles. Morphological analysis of the as prepared samples was carried out by field emission scanning electron microscopy (FESEM). Confocal Raman imaging has been studied and an attempt has been made to find out the graphitic ( ) and disordered phase of the CNTs.