This study investigated the effects of oxygen (O2) flow rates and annealing temperatures on optical, electrical, and structural properties of indium–gallium–zinc oxide (IGZO) film on glass substrates fabricated by using a co-sputtering system with two radio-frequency (RF) (In2O3 and Ga2O3) and one direct current (DC) (Zn) magnetron. The average transmittance and optical energy gap increased significantly when the oxygen flow rate was increased from 1 sccm to 3 sccm. An increased O2 flow during co-sputtering IGZO films caused the crystallinity of the InGaZn7O10 phase to increase, yielding a smoother and more uniform granular structure. The carrier mobility rose and the carrier concentration decreased with increasing O2 flow. The results of X-ray photoelectron spectra (XPS) analyses explained the impacts of the O2 flow rates and annealing temperatures on optical and electrical properties of the co-sputtered IGZO films. The optimum process conditions of the co-sputtered In2O3-Ga2O3-Zn films were revealed as an O2 flow rate of 3 sccm and an annealing temperature at 300 °C, which showed the largest average transmittance of 82.48%, a larger optical bandgap of 3.21 eV, and a larger carrier mobility of 7.01 cm2 V−1s−1. XPS results at various annealing temperatures indicated that the co-sputtered IGZO films with an O2 flow rate of 3 sccm have more stable chemical compositions among different annealing temperatures.
9 July 2016 in Journal of Materials Science: Materials in Electronics
In this study, indium–tin oxide (ITO)/Nb-doping TiO2 (TNO) double-layer transparent conductive oxide (TCO) films deposited using DC magnetron sputtering were used as a surface anti-reflection layer with an overall thickness of 100 nm for double-layer films. The simulated results showed that ITO and TNO thickness combinations of 90 nm/10 nm, 80 nm/20 nm, and 70 nm/30 nm had a higher transmittance and lower reflectance than others in the visible wavelength range. Compared to the single-layer ITO films, for ITO/TNO films deposited on the glass and silicon substrates with an optimum thickness of 80/20 nm, the reflectance was reduced by 5.06% and 4.63%, respectively, at the central wavelength of 550 nm and crystalline silicon photo response wavelength of 900 nm. Moreover, the near-infrared reflectance of the double-layer ITO/TNO with thickness combinations of 90 nm/10 nm, 80 nm/20 nm, and 70 nm/30 nm, when deposited on silicon substrates, was obviously improved by the graded refractive index lamination effect of air (1)/ITO (1.98)/TNO (2.41)/Si (3.9).
In this work, two stacked gate dielectrics of Al2O3/tetraethyl-orthosilicate (TEOS) oxide were deposited by using the equivalent capacitance with 100-nm thick TEOS oxide on the patterned InGaZnO layers to evaluate the electrical characteristics and stability improvement of amorphous indium gallium zinc oxide (a-IGZO) thin-film transistors (TFTs) devices, including positive bias stress (PBS) and negative bias stress (NBS) tests. Three different kinds of gate dielectrics (Al2O3, TEOS, Al2O3/TEOS) were used to fabricate four types of devices, differing by the gate dielectric, as well as its thickness. As the Al2O3 thickness of Al2O3/TEOS oxide dielectric stacks increased, both the on-current and off-current decreased, and the transfer curves shifted to larger voltages. The lowest ∆Vth of 0.68 V and ∆S.S. of −0.03 V/decade from hysteresis characteristics indicate that the increase of interface traps and charge trapping between the IGZO channel and gate dielectrics is effectively inhibited by using two stacked dielectrics with 10-nm thick Al2O3 and 96-nm thick TEOS oxide. The lowest ∆Vth and ∆S.S. values of a-IGZO TFTs with 10-nm thick Al2O3 and 96-nm thick TEOS oxide gate dielectrics according to the PBS and NBS tests were shown to have the best electrical stability in comparison to those with the Al2O3 or TEOS oxide single-layer dielectrics.
The optical, electrical, and material properties of In–Zn–O (IZO) films were optimized by adjusting the deposition power and annealing temperature. Films deposited at 125 W and annealed at 300 °C exhibited the best performance, with the lowest resistivity (1.43 × 10−3 Ω·cm), highest mobility (11.12 cm2/V·s), and highest carrier concentration (4.61 × 1020 cm−3). The average transmittance and optical energy gap were 82.57% and 3.372 eV, respectively. The electrical characteristics of amorphous In-Ga-Zn-O (a-IGZO) thin-film transistors (TFTs) using IZO source-drain (S–D) electrodes with various sputtering powers and annealing temperatures were investigated. The optimal sputtering power of 125 W and annealing temperature of 300 °C for the IZO S–D electrodes resulted in the highest field-effect mobility (~12.31 cm2/V·s) and on current (~2.09 × 10−6 A). This improvement is attributed to enhanced carrier concentration and mobility, which result from the high In/Zn ratio, the larger grain size, and low RMS roughness in the IZO films. The parasitic contact resistance (RSD) and channel resistance (RCH) were analyzed using the total resistance method. RSD decreased with increasing IZO S–D sputtering power, while RCH reached a minimum at 125 W. Both resistances decreased significantly as the annealing temperature increased from 200 °C to 300 °C.
28 April 2014 in Japanese Journal of Applied Physics
In this study, we have successfully fabricated In–Ga–Zn–O (IGZO) thin-film transistors (TFTs) with various Ga2O3 deposition powers prepared using a two radio-frequency (RF) (ceramics targets: In2O3 and Ga2O3) and one direct-current (DC) (metallic target: Zn) magnetron cosputtering system at room temperature. The carrier concentration for the IGZO films decreases to less than 3 × 1016 cm−3 when the Ga2O3 deposition power is 175 W and Hall mobility decreases from 12.8 cm2 V−1 s−1 and saturates at 4.6 cm2 V−1 s−1 with increasing Ga2O3 deposition power. The increase in the resistivity of the cosputtered films correlates with the decrease in the crystallinity of the InGaZn7O10 phase and the phase transformation from InGaZn7O10 to InGaZn2O5 with increasing Ga2O3 deposition power. With an optimum Ga2O3 deposition power of 150 W, cosputtered IGZO TFTs with a higher, saturated drain current of 4.5 µA, good saturation mobility, μsat of 4.92 cm2 V−1 s−1, Ion/Ioff of 109, a low subthreshold swing (SS) of 0.27 V/decade, and RSD of 30 kΩ have been successfully fabricated.