The Nafion films from ethanol-diluted Nafion dispersions of concentration 0.5 wt% were deposited on mica substrate by spin coating. The thickness of the film was 1 ± 0.2 nm measured with surface force apparatus techniques in dry nitrogen. Due to the swelling of Nafion in water, the thickness of the film increased to 4.8 ± 1 nm. The thickness had a sudden jump-in with high load (40 mN/m) in water, possibly because a few layers of water molecules were extruded from the Nafion film. The surface topography of the Nafion film pretreated with the Nafion solution the same as that used in the SFA experiments was characterized by atomic force microscopy (AFM). The Nafion polymers formed a relatively uniform region in two-dimension on the mica substrate via spin coating. The completely repulsive force at all distances between Nafion and mica surface indicates that the surface of Nafion is negative in water.