Background. The effect of beverages on nanocomposite denture base materials is neglected. Therefore, this study aimed to investigate the influence of different beverages (coffee, tea, cola, and mineral water) on the color stability of nanoparticles-modified denture base materials (DBMs). Materials and Methods. A total of 280 specimens (n = 10/group) were prepared from heat-polymerized acrylic resin modified with different concentrations (3% and 7%) of zirconium dioxide (nano-ZrO2), titanium dioxide (nano-TiO2), and silicon dioxide (nano-SiO2) nanoparticles, while 0% was taken as a control. Color change (∆E) of the specimens was evaluated after simulating 6-month immersion time in four commonly used beverages, coffee, tea, cola, and mineral water, as experimental groups. Color stability was measured using a spectrophotometer, and then values were converted to National Bureau of Standards units (NBS units). The one-way ANOVA test was applied to compare color change (ΔE) results followed by Bonferroni’s post hoc test (α = 0.05). Results. The results showed that the heat-polymerized acrylic resin modified with different types of nanoparticles showed lower color changes after being immersed in beverage solutions compared to the unmodified group ( < 0.001), so the color stability of heat-polymerized acrylic resin was significantly enhanced by the addition of several nanoparticles; nano-ZrO2 showed the lowest ΔE followed by nano-TiO2 and then nano-SiO2. Regardless of the filler type, 3% concentration showed lower mean ΔE than 7% concentration. Regarding the beverage solutions, the greatest color change was found in the coffee group followed by tea and cola, while water showed the least changes. Conclusion. Modification of heat-polymerized acrylic resin with certain amounts of nano-ZrO2, nano-TiO2, and nano-SiO2 may be useful in improving color stability.
To evaluate the effect of beverages (coffee, tea, Cola-Cola, and mineral water) on the color stability of resin-based composite (RBC) materials modified with different nanoparticles (NPs). The specimens (70/beverage) were fabricated from light-cured RBCs and divided according to NPs into four groups: one control, unmodified (N0); and three experimental—ZrO2 (Zr), TiO2 (Ti), and SiO2 (Si) groups. Each experimental group was further subdivided into two subgroups according to NP concentrations: 3 wt.% and 7 wt.% (n = 10). A spectrophotometer was used to assess the color change (∆E) before and after six months of immersion. Data were analyzed and compared using one-way-ANOVA followed by Bonferroni’s post-hoc test (α = 0.05) and subsequently ∆E value conversion to National Bureau of Standards (NBS) units. The modified light-cured RBCs with ZrO2, TiO2, and SiO2 demonstrated smaller color changes after immersion in the beverages than the unmodified group (p < 0.001). Zr groups showed the lowest ΔE, followed by Ti and Si groups; a 3% concentration resulted in a lower mean ΔE than the 7% concentration. NBS findings showed that coffee and tea produced marked unacceptable color changes (NBS units were >3), and Coca-Cola resulted in noticeable color changes (NBS units between 1.5 and 3), while water produced slight color changes (NBS ≤ 1). Modification of RBCs with both concentrations of ZrO2, as well as 3% of TiO2 and SiO2, may improve its color stability. Based on NBS results, RBCs immersed in mineral water and Coca-Cola showed clinically acceptable color changes, while those immersed in coffee and tea were clinically unacceptable.
29 April 2023 in International Journal of Dentistry
Background. Although the mechanical behaviors of PMMA were improved with nanoparticles addition, there is a lack of study on the color changes of nanocomposite denture base resin. This study aimed to assess and compare the color of nanocomposite denture base resin modified with different nanoparticles and concentrations. Materials and Methods. Three nanoparticles (zirconium dioxide (ZNP), titanium dioxide (TNP), and silicon dioxide (SNP)) were added to heat-polymerized acrylic resin in 3 and 7 wt% concentrations. A total of 70 acrylic discs (20 × 2 ± 0.03 mm) specimens were prepared while one without addition (control) and three main groups according to nanoparticles and two subgroups according to % (3ZNP, 7ZNP, 3TNP, 7TNP, 3SNP, and 7SNP) with total 70 acrylic discs (n = 10). Spectrophotometer was used for color change (ΔEab) followed by value conversion to National Bureau of Standards units (NBS) to relate the color alterations (ΔEab) to the clinical environment which aids in determining a threshold for clinical acceptance of the color change. ΔEab data were analyzed and compared using one- and two-way ANOVA tests followed by Bonferroni’s post hoc test (α = 0.05). Results. Two-way ANOVA showed that filler type (regardless of filler concentration) had a statistically significant effect on mean ΔEab ( ). Filler concentrations (regardless of filler type) showed a significant effect on mean ΔEab while the filler type and concentration interaction showed no significant effect on mean ΔEab ( ). One-way ANOVA in terms of filler types results showed a significant difference between mean ΔEab ( ), where TNP group showed the highest mean ΔEab followed by ZNP and SNP. Pair-wise comparison revealed that 3% concentration showed a significant lower mean ΔEab than 7% concentration ( ). Conclusion. Modification of heat-polymerized denture base resin with ZNP, TNP, or SNP causes clinically unacceptable color change. TNP produced the highest color change followed by ZNP and SNP, and the color change is concentration dependent; the color change increases as the concentration increases.