The alloy powder and SiCw reinforcement were ball milled, cold-pressed, sintered, hot extruded and solution aged to obtain excellent mechanical properties such as hardness and compressive strength. The microstructure and properties of the material were characterized by metallographic microscope, scanning electron microscope (SEM), EDS, X-ray diffraction (XRD), HV-1000 microhardness and 7051 eddy current conductivity. The results show that the distribution of SiC whiskers in the mixed powder is relatively uniform, but there is still a small amount of agglomeration phenomenon in the sintered sample. The optimum cold pressure is 740 MPa. With the increase in SiCw content, the hardness, dislocation density and compressive strength of aluminum matrix composites are improved. The compressive strength of 5%SiCw reinforced aluminum matrix composite is 658.9 MPa and the elongation is 6.7%.
A mixture of the Ti-Mo-Nb-Al-Si matrix powder and Carbon nanotubes (CNTs) particles were used as the raw powder to produce the in-situ TiC reinforced titanium matrix composites (TMCs) via powder metallurgy. The effects of various contents of CNTs on the microstructure, phase composition and hot corrosion behavior of the composites were investigated. The results show that the corrosion mass gain of the composites with CNTs content of 1.0 wt.% was the minimum (18.73 mgcm-2), which was about 44.4% lighter than that of the matrix (33.70 mgcm-2). XRD results show that the corrosion phases were mainly composed of TiO2, Al2O3, SiO2, Ti(SO4)2, NaTiO2 and TiS. According to the SEM results, the grain size of the as-sintered composites can be refined by adding CNTs. With the increase of CNTs content, the grain size became smaller and smaller. The cross-sectional morphology shows that the oxide layer of the composites with 1.0 wt.% CNTs after corrosion was denser and thinner (21.44 μm). It was about 82.13% thinner than the oxide layer of the matrix (120.00 μm). All the results show that the TMCs with 1.0 wt.% CNTs have better hot corrosion resistance.
In this paper, Al-11.1Zn-2.7Mg-1.7Cu-1.4Ti-0.2Zr alloy material was prepared by powder metallurgy to study the effect of the different solid-solution aging systems on the microstructure and mechanical properties of this 7000 series aluminum alloy. The microstructure of the alloy under the three different solid-solution processes S1, S2, and S3 were observed using an optical microscope, scanning electron microscope, and X-ray diffraction analysis. The mechanical properties were tested to determine the best solid-solution process. The results show that under the S2 solid-solution process, the alloy has the best mechanical properties, with a compressive strength of 646.7(±6.5) MPa and a fracture strain of 5.9(±0.06)%. The maximum hardness trends in the three solid-solution processes after aging are S2>S3>S1. The maximum hardness 220.7(±5.5 )HV occurs after S2 solid-solution and 121℃×18 h aging. Moreover, after S2 solid-solution treatment, the solid-solution degree is close to saturation, the solid-solution strengthening effect is the best, and dislocations contribute the most to the strength.
The paper discusses the effects of B4C particle (B4Cp) content on the microstructure and high-temperature oxidation resistance of B4Cp/Ti-5.4Al-4.03Mo-3.93V-2.37Cr-0.01Zr composite prepared by powder metallurgy. The results demonstrate that grain size of the composites decreases by increasing reinforcement content from 1 to 3 wt.%, suggesting that B4Cp can refine grain of the materials. For the composites with increasing B4Cp content from 0 to 3 wt.%, the apparent porosity increase from 3.23 to 6.89%, indicating that the density of materials decreased with the increase of B4CP content. In addition, the hardness of the materials have been greatly improved. Comparing to the substrate 434.02 HV, the 1, 2, and 3 wt.% B4CP specimens are increased by 37.2%, 57.5%, and 84.7%, respectively. The weight of the oxidation product is reduced and the oxidation rate is slowed down, as the B4CP content increases. Moreover, the thickness of the oxide layer is greatly reduced, and the thickness of oxidation layer in composites with 0, 1, 2 and 3 wt.% B4CP specimens were 60, 55, 47 and 40 μm, indicating that B4CP can improve the high-temperature oxidation resistance.