A composite membrane was fabricated from biopolymer chitosan and montmorillonite (MMT) filler as an alternative membrane electrolyte for direct methanol fuel cell (DMFC) application. To first improve the organic–inorganic interfacial morphology, the pristine MMT was pre-treated using 3-glicidoxy propyltrimethoxysilane (GPTMS) surface modifier to produce organophilic MMT (O-MMT). The GPTMS modified MMT was mixed with chitosan in acetic acid solution and cast into membranes. SEM images and FTIR analysis showed that the O-MMT was successfully incorporated into the chitosan polymer matrix. Water and methanol uptake of the Ch/O-MMT composite membranes decreased with increasing O-MMT loadings, but the ion exchange capacity (IEC) value increased. The Ch/O-MMT with 5 wt% O-MMT loading exhibited the best methanol permeability and proton conductivity characteristics among the other Ch/O-MMT membranes, which were 3.03 × 10−7 cm2 s−1 and 4.66 mS cm−1, respectively. All the results obtained from this study can be used to conclude that the chitosan membrane with O-MMT filler is a promising high performance PEM candidate for DMFC application.
In this study, chitosan (CS) doped sulphosuccinic acid (SSA)–glycerol (Gly) and modified montmorillonite clay (MMT) were successfully fabricated. The membranes were prepared using the solution casting method. Analysis of morphology and topography using scanning electron microscopy (SEM) and atomic force microscopy (AFM) revealed that the composite membrane with 3 wt% MMT filler, namely CS/MMT-1, possessed the most adequate surface roughness compared to the other fabricated membranes. Furthermore, mechanical characterization of the CS/MMT-1 composite membrane showed that the membrane achieved satisfactory mechanical strength with a value of 39.23 MPa. Proton conductivity of the composite membranes increased as the temperature was increased. The proton conductivity of the CS/MMT-1 composite membrane increased from 1.75 × 10−2 S cm−1 at 25 °C up to 3.57 × 10−2 S cm−1 at 80 °C. The CS/MMT-1 composite membrane also exhibited a methanol permeability value that was significantly lower than that of pristine CS, namely 1.22 × 10−7 cm2 s−1 and 12.49 × 10−7 cm2 s−1, respectively. The results of this study show that the fabricated composite membrane can be used as an alternative polymer electrolyte membrane (PEM) for DMFC applications.
The development of active anode material derived from Southeast Celebes with chitosan-PVA binder is one of the alternatives to change the graphite anode on Lithium ion batteries. Anode is composed by hematite that is extracted from the dissolution of natural iron sand with strong acid and chitosan is derived from shrimp shell waste. The composition of the active material, binder, and conductive material on the anode were varied 57.14 : 28.56 : 20 and 60 : 20 : 20 (%w/w), respectively. Characterizations using FTIR, XRD, and SEM were conducted to determine physical properties of extracted material. Performance tests on the anodes that have been assembled in lithium ion batteries included EIS, CV, and CD. The optimal composition is 60:20:20 (%w/w) with EIS and CD results of 1069 Ω and 420 mAh/g, repectively. The CV results have shown a reduction potential at 0.503 V and an oxidation potential of 1.803 V. The local iron sand of Southeast Sulawesi can be used as a source of the active material on the anode.