Aqueous dispersions of gold and silver nanoparticles (NPs) stabilized with sodium citrate, as well as polymeric NPs based on poly(lactide- co -glycolide) (70 : 30 mol %) stabilized with poly(vinyl alcohol) have been obtained. The sizes of NPs have been determined by transmission electron microscopy (TEM), dynamic light scattering (DLS), and analytical ultracentrifugation (AUC). It has been shown that the diameter of both metallic and polymeric particles measured by TEM is significantly lower than their hydrodynamic diameter Dh determined by DLS. Moreover, it has been found that the Dh value obtained for the studied particles from DLS distributions is overestimated compared to that determined by AUC, because the AUC method is less sensitive to the particle size polydispersity and the presence of large objects in a dispersion.
The kinetic of D,L‐lactide polymerization in presence of biocompatible zirconium acetylacetonate initiator was studied by differential scanning calorimetry in isothermal mode at various temperatures and initiator concentrations. The enthalpy of D,L‐lactide polymerization measured directly in DSC cell was found to be ΔH=−17.8±1.4 kJ mol−1. Kinetic curves of D,L‐lactide polymerization and propagation rate constants were determined for polymerization with zirconium acetylacetonate at concentrations of 250–1000 ppm and temperature of 160–220 °C. Using model or reversible polymerization the following kinetic and thermodynamic parameters were calculated: activation energy Ea=44.51±5.35 kJ mol−1, preexponential constant lnA=15.47±1.38, entropy of polymerization ΔS=−25.14 J mol−1 K−1. The effect of reaction conditions on the molecular weight of poly(D,L‐lactide) was shown.
В работе проводится исследование спектров комбинационного рассеяния (КР) света ряда материалов на основе полилактида: стереоизомеров полилактида, олигомеров L-лактида, сополимеров L-лактида и ε-капролактона, композитов поли(L-лактида) и гидроксиапатита. Установлено, что по спектрам КР можно определять состав и степень кристалличности широкого круга материалов на основе полилактида. Развитие такой методики очень важно для разработки инновационных материалов на основе полилактида, используемых как для разнообразных медицинских применений, так и, например, при создании биоразлагаемой одноразовой упаковки для решения проблем загрязнения окружающей среды.
Kinetics of polymerization of ε-caprolactone initiated by zirconium acetylacetonate Zr(acac)4 in the presence of ethylene glycol as a co-initiator was studied. Detailed kinetic analysis was performed using Friedman differential isoconversional method in combination with analysis of the enthalpy–entropy compensation effect, resulting in model-free evaluation of the kinetic triplet of the reaction: \({{E}_{{{\alpha }}}}\), \({{A}_{{{\alpha }}}}\), and \(f\left( {{\alpha }} \right)\). In addition, the activation energy \({{E}_{{{\alpha }}}}\) was calculated using the first-order reaction model. The obtained value \({{E}_{{{\alpha }}}}\) = 65.5 ± 2.3 kJ/mol was consistent with the average \({{E}_{{{\alpha }}}}\) values calculated by the isoconversional method. It was shown that the sigmoidal nature of polymerization is adequately described by the Kamal autocatalytic model. The effect of reaction temperature and initiator concentration on the molecular-weight characteristics of resulting poly(ε-caprolactone) was investigated. When the reaction temperature is 100–140°C, the molecular weight of the polymer is Mn ≈ 40–50 kDa and the dispersity is Ð ≈ 1.7–2.0.