Reducing charge carrier transport losses, improving selectivity, and minimizing nonradiative recombination are essential for enhancing the efficiency and stability of perovskite/silicon tandem solar cells. We used a hybrid two-step perovskite deposition method that is compatible with industry-standard textured silicon, incorporating a perovskite surface treatment based on 1,3-diaminopropane dihydroiodide. The interaction of this molecule with the perovskite surface increased the majority charge carrier concentration at the electron-selective contact, which reduced interfacial recombination. Simultaneously, this field-effect passivation increased the electron concentration across the entire intrinsic perovskite absorber, which increased conductivity and reduced transport losses. Combined, this yields high-performance, fully textured perovskite/silicon tandem solar cells, achieving a 1-sun AM1.5G conversion efficiency of 33.1% with an open-circuit voltage of 2.01 volts and an extended outdoor stability in the Red Sea Coast.
27 November 2017 in Progress in Photovoltaics: Research and Applications
With the surge of UV‐transparent module encapsulants in the photovoltaic industry aiming to boost quantum efficiency, modern silicon solar cells must now inherently withstand UV exposure. UV‐induced degradation (UVID) of nonencapsulated laboratory and industrial solar cells from several manufacturers is investigated. Passivated emitter rear contact (PERC), tunnel oxide passivating contact (TOPCon), and silicon heterojunction (HJT) cells can suffer from severe implied voltage degradation (>20 mV) after UV exposure relating to 3.8 years of module installation in the Negev desert. Front UV‐exposure causes more performance loss than an equal rear dose. This is connected to a higher UV transmission of the cell layers outside the bulk, indicating the photons need to reach the silicon surface to induce damage. Current–voltage measurements of the TOPCon groups most sensitive to UV degradation show more than 7%rel efficiency loss with the Voc as the main contributor. For two TOPCon groups, dark storage for 14 days after UV exposure causes an additional voltage drop on a similar scale as the UV damage itself, impeding straightforward reliability testing. UVID appears to be a complex process general to all dominant cell architectures with the potential to diminish efforts in efficiency optimization within only a few years of field employment.
In this article, the impact of different hydrogen configurations and their evolution on the extent and kinetics of light- and elevated-temperature-induced degradation (LeTID) is investigated in float-zone silicon via charge carrier lifetime measurements, low-temperature Fourier-transform infrared spectroscopy, and four-point-probe resistance measurements. Degradation conditions were light soaking at 77 °C and 1 sun-equivalent illumination intensity and dark anneal at 175 °C. The initial configuration of hydrogen is manipulated by varying the wafer thickness, the cooling ramp of the fast-firing process, and the dopant type (B- or P-doped). We find lower hydrogen concentrations in thinner samples and samples with a slower cooling ramp. This suggests that hydrogen diffuses out of the sample during the cool-down, which strongly affects the final concentration of hydrogen molecules H 2 , and to a smaller degree the concentration of boron-hydrogen (BH) pairs. A regeneration of potential LeTID defects and a presumed LeTID degradation during dark annealing is found in n-type Si. In p-type Si, the LeTID extent was found to scale with H 2 , suggesting a direct link between both. The temporal evolution of BH pairs, LeTID degradation/regeneration, and surface degradation depends on wafer thickness and the cooling ramp of the fast-firing process. Based upon these findings, we formulate a theory of the hydrogen-related mechanism behind LeTID: Hydrogen originating from H 2 moves between different temporary traps. First, hydrogen binds to LeTID precursors and acceptor atoms in the silicon bulk, later moving toward the surface. This leads first to the LeTID degradation and regeneration and then to the degradation of surface passivation.
We present an overview of imaging techniques for analyzing different loss mechanisms in solar cells. The bulk and surface recombination, optical, series resistance, and shunt losses are investigated in more detail. It is shown that a detailed spatially resolved analysis of these loss channels is possible by combining different evaluation methods. Photoluminescence imaging is used to analyze carrier recombination in the material volume and the surfaces. Bulk recombination is investigated on wafer level by an analysis, which is able to investigate the impact of bulk lifetime and impurity concentration on cell efficiency. Variations in the production conditions of multicrystalline silicon serve as an example. Surface recombination is investigated on a cell precursor level, and the importance of detecting surface defects in cell processes featuring dielectric rear-side passivation is highlighted. For analyzing optical, series resistance, and shunt losses on final cells, a combination of photoluminescence imaging, dark lock-in thermography, and spectrally resolved light-beam-induced current is proposed. As an example, a detailed analysis of two solar cells is presented, allowing the assessment of the local and global impact of each loss mechanism on cell efficiency.
27 November 2023 in Progress in Photovoltaics: Research and Applications
As the efficiency of perovskite silicon tandem solar cells is increasing, the upscaling for industrial production is coming into focus. Spatially resolved, quantitative, fast, and reliable contactless measurement techniques are demanded for quality assurance and to pinpoint the cause of performance losses in perovskite silicon tandem solar cells. In this publication, we present a measurement method based on spectrally integrated photoluminescence (PL) imaging to extract subcell‐selective implied open‐circuit ( ) images from monolithic perovskite silicon tandem solar cells. We validate the approach using spectrally resolved absolute PL measurements based on an integrating sphere for the perovskite top cell and PL‐calibrated carrier lifetime images for the silicon bottom cell. Additionally, measurements of solar cells with low contact losses are used to validate the new measurement technique. We find a good agreement of the images with the validating measurements with a maximum deviation of well below 1% compared to the validation measurements.