The depletion of the ore reserves in the world necessitates the search for secondary sources such as waste products (tailings and slag). The treatment and cleaning up of such secondary sources also has a positive impact on the environment. A smelter in Namibia we examined had historic slag which accumulated over decades of its operating life, thus posing the challenge of how best to collect representative samples to evaluate and propose viable methods of recovering contained metals. In this study, analytical and mineralogical characterization of the slag was performed using X-ray fluorescence (XRF) analysis, atomic absorption spectrometer (AAS), ICP-OES, scanning electron microscopy energy dispersive spectroscopy (SEM-EDS) analysis, and optical microscopy analysis. The chemical analyses showed that the metal values contained in the slag were mainly copper, lead, and zinc whose average contents were approximately 0.35% Cu, 3% Pb, and 5.5% Zn. About 10.5% Fe was also contained in the slag. Germanium was detected by scanning electron microscopy, but was however below detection limits of the chemical analysis equipment used. Based on the results, approximate conditions under which the different slag phases were formed were estimated and the recovery routes for the various metals were proposed. Analysis by both optical and scanning electron microscopy revealed that Zn and Fe occurred mainly in association with O as oxides, while Cu and Pb were mainly associated with S as sulphides. The slag consisted of three different phases, namely the silicate phase (slag), metallic phase and the sulphide phases. The phases in the slag were mainly silicate phases as well as metallic and sulphide phases. It was observed that the metallic and sulphide phases were dominant in the finer size fractions (−75 µm) whereas the sulphide phase was also present in the coarser size fractions (+300 µm). An important finding from the microscopy examination was that the sulphide phases were interstitial and could be liberated from the slag. This finding meant that liberation and subsequent concentration of the sulphide phases was feasible using conventional processing techniques.
14 April 2023 in Journal of the Southern African Institute of Mining and Metallurgy
The effect of mineralogy on the grindability was investigated using three copper ores - two sulphides and one oxide. The dominant copper minerals were identified by optical microscopy and mineral chemistry derived from SEM-EDS analysis. The sample designated sulphide 1 was bornite-rich, sulphide 2 ore was mainly chalcopyrite, and the oxide ore was predominantly malachite and minor azurite. The gangue minerals were identified using semi-qualitative XRD analysis. Sulphide 1 contained more than 80% (w/w) of quartz compared to about 70% in the other two ores. The Bond work indices were 13.8, 21.6, and 17.3 kWh/t for sulphide 1, sulphide 2, and oxide ore respectively. This suggested that the chalcopyrite-rich ore is the hardest, while the malachite-rich ore has intermediate hardness, and the bornite-rich ore is the softest. The brittleness indices of the ores were calculated using the chemical composition of the gangue, and a good correlation between brittleness indices and Bond work indices was observed, which highlights the importance of the gangue composition in determining the fracture behaviour of the ores. There is scope for further investigation into the relationship between ore mineralogy and comminution behaviour using other breakage characterization techniques.
The depletion of the ore reserves in the world necessitates the search for secondary sources such as waste products (tailings and slag). A smelter in Namibia has historic slag which accumulated over decades of its operating life. Analytical and mineralogical characterization of the slag was performed using the X-ray fluorescence (XRF) analysis, Atomic Absorption Spectrometer (AAS), ICP-OES, scanning electron microscopy energy dispersive spectroscopy (SEM-EDS) analysis, and optical microscopy analysis. The chemical analyses showed that the metal values contained in the slag were mainly copper, lead, and zinc whose average contents were approximately 0.3%Cu, 2.4%Pb and 3.2%Zn. About 10.5%Fe was also contained in the slag. Germanium was detected by scanning electron microscopy, but was however below detection limits of the chemical analysis equipment used. Based on the results, approximate conditions under which the different slag phases were formed were estimated and the recovery routes for the various metals were proposed. Analysis by both optical and scanning electron microscopy revealed that Zn and Fe occurred mainly in association with O as oxides, while Cu and Pb were mainly associated with S as sulphides. The slag consisted of three different phases; namely the silicate phase (slag), metallic phase and the sulphide phases. The slag phases were mainly glass, silicate phases and metallic and sulphide phases. It was observed that the metallic and sulphide phases were dominant in the finer size fractions (-75 µm) whereas the sulphide phase was also present in the coarser size fractions (+300 µm). An important finding from the microscopy examination was that the sulphide phases were interstitial and could be liberated from the slag. This finding meant that liberation and subsequent concentration of the sulphide phases was feasible using conventional processing techniques.
The study evaluated the milling kinetics of three copper ores, from a multi-mineralised deposit, which were identified as sulphide 1 (with bornite as a dominant copper mineral), sulphide 2 (mainly composed of chalcopyrite) and oxide (with malachite as a dominant copper mineral) and related the breakage parameters to the mineral composition data. Five mono-size fractions between 1000 µm and 212 µm were dry milled for short grinding times in the laboratory ball mill in order to obtain data for predicting breakage rate parameters. The analytical and mineralogical characterisation of the ores were performed using X-ray fluorescence (XRF) analysis, scanning electron microscopy energy dispersive spectroscopy (SEM-EDS) analysis, optical microscopy analysis and X-ray diffractometer (XRD). The mineralogy data showed that quartz was the abundant gangue mineral (average for each ore was above 60% (w/w)), followed by K-feldspar minerals (orthoclase and microcline) which constituted between 4% (w/w) and 6% (w/w) and the remainder are the minor calcite and dolomite minerals which are also in the host rock. The experimental milling kinetics parameters and mineralogical data were used to assess the robustness of the heterogeneous (two-component) and homogeneous (single-component) first-order rate breakage models. The mineral composition data were used for setting up the predictions of breakage parameters in the two-component and single-component first-order breakage models. The experimental data fitted better on the two-component breakage model than the single-component breakage model. These results highlighted the influence of two groups of minerals (generally classed as valuable and gangue minerals). The breakage data showed that the selection function for the hard component (the gangue minerals) has a dominant contribution to the overall selection function of the ores, with SiA correlating fairly well with experimental Si. The parameter a in the Austin empirical breakage model was relatively similar (approximately 1) for all three ores, which confirms similar milling conditions to which the ores were subjected to. The data suggests that there is a relationship between breakage parameter α (material-specific parameter) in the Austin empirical breakage model and brittleness index βi (calculated from the mineralogical composition of the gangue phase). No clear trends could be deduced from the cumulative breakage distributions of the three ores. This highlights the complexity of developing relationships between the mineralogical composition data and breakage distributions of the ores which are extracted from the same deposit and with comparable gangue composition.
The old tailings from mine dumps in Namibia contain not only copper but also precious metals and other metal values, such as lead and zinc, which should be recovered to supplement the production of metals from ores. X-ray fluorescence (XRF) analysis of the tailings showed that it contained 0.8% Cu, 40 ppm Au, 60 ppm Ag, 0.9% Pb, 0.7% Zn and 1% Fe. Batch roughing tests were conducted to investigate the effect of pH, collector (PAX) dosage, and sulphidiser (Na2S) dosage on the recovery of copper and precious metals (Ag and Au). Results for flotation test work showed that recovery of metal values depends on the three operating variables. Maximum recoveries of Cu (52%), Ag (53%) and Au (44%) were achieved at pH 10.5, PAX dosage of 47 g/t, Na2S dosage of 109 g/t and 12-minute residence time. Testwork is still in progress to improve the recoveries of copper, gold and silver.
The reprocessing of metallurgical wastes to recover much-needed metals such as copper not only ensures an adequate supply of metals but also contributes to the cleaning of the environment. A copper smelter in Namibia accumulated significant amounts of spent refractory bricks that are enriched with metal values including copper. This supposedly waste material can potentially serve as a supplement to the ore concentrate, as a smelter feedstock for this toll smelter. Representative samples of crushed bricks, designated as Sample 1 and Sample 2, were used for mineralogical characterisation and flotation test work. The assays for Sample 1 and Sample 2 were 14% Cu and 18% Cu, respectively. Microscopy results identified various copper phases including metallic Cu, bornite, malachite and chalcopyrite. Batch flotation tests were conducted to investigate the effect of grind size (P80 of 53, 75 and 106 μm), pulp pH (natural pulp pH, 10, 10.5 and 11) and collector (potassium amyl xanthate, PAX) dosage (70, 100 and 130 g/t) on the recovery of copper, concentrate grade and weight recovery. In some tests, a co-collector (dithiophosphate, DTP) and sulphidiser (Na2S) were also added in the quest to maximise the recovery of copper. Based on the test conditions investigated in this study, the grind size is the key variable affecting the recovery of copper. The best copper recovery of 86% (with a weight recovery in the range of 42 to 45% (w/w) and concentrate grade of 37% Cu) was achieved for the finest grind size of 53 μm. The reagent suite that yielded the best recovery was 70 g/t PAX with no addition of the sulphidiser while the pH was 10. There is scope for developing the process routes to recover other valuable metals such as iron, lead and zinc that are also in the spent bricks, as well as potential reuse of the spent bricks (after recovering valuable metals) to make new refractory bricks.