With continuous improvements, structural steels are available in even higher strength grades above 1000 MPa yield strength. As the great majority of these steels are used in welded structures, their weldability needs to be taken into account. Several factors can cause difficulties during welding of these steels, but in this paper the softening behavior and the toughness characteristics of the heat-affected zone (HAZ) are examined. As the critical parts of the HAZ in a real welded joint are relatively small, their investigating ability is limited. However, the physical simulation provides a way of evaluating specimens made from a given material to produce the specified HAZ areas in a suitable size range for subsequent testing. In this research work, three different strength categories of high-strength structural steels (with yield strength of 960 MPa, 1100 MPa, and 1300 MPa) are investigated by physical simulation. In the case of different technological variants of gas metal arc welding (GMAW) process, the effect of the cooling time t8/5 is investigated in different HAZ subzones considered to be critical. The thermal cycles were determined according to the Rykalin 3D model. The investigated cooling times were t8/5 = 5 s, 15 s, and 30 s. The properties of the selected coarse-grained, intercritical and intercritically reheated coarse-grained zones are analyzed by laser scanning microscope, scanning electron microscope, hardness test, and instrumented Charpy V-notch impact toughness test. Furthermore, additional investigation like JMatPro calculations, electron backscatter diffraction measurements, and prior austenite grain size calculation were carried out. As a result of the tests, the investigated heat-affected subzones indicated higher sensitivity to the welding heat input compared to conventional structural steels. Overall, the results of the tests show that the application of shorter t8/5 cooling time can be beneficial for the investigated high-strength steel grades, since significant toughness reduction and the risk of softening occur in the whole cooling time range.
The presence of acicular ferrite (AF) in the heat-affected zone (HAZ) of steels used offshore is generally seen as beneficial for toughness. In this study, the effects of varying fractions of AF (0–49 vol.%) were assessed in the simulated, unaltered and coarse-grained heat-affected zones (CGHAZ) of three experimental steels. Two steels were deoxidized using Ti and one using Al. The characterization was carried out by using electron microscopy, energy-dispersive X-ray spectrometry, electron backscatter diffraction and X-ray diffraction. The fraction of AF varied with the heat input and cooling time applied in the Gleeble thermomechanical simulator. AF was present in one of the Ti-deoxidized steels with all the applied cooling times, and its fraction increased with increasing cooling time. However, in other materials, only a small fraction (13–22%) of AF was present and only when the longest cooling time was applied. The impact toughness of the simulated specimens was evaluated using instrumented Charpy V-notch testing. Contrary to the assumption, the highest impact toughness was obtained in the conventional Al-deoxidized steel with little or no AF in the microstructure, while the variants with the highest fraction of AF had the lowest impact toughness. It was concluded that the coarser microstructural and inclusion features of the steels with AF and also the fraction of AF may not have been great enough to improve the CGHAZ toughness of the steels investigated.
Deterioration of the toughness in heat-affected zones (HAZs) due to the thermal cycles caused by welding is a known problem in offshore steels. Acicular ferrite (AF) in the HAZ is generally considered beneficial regarding the toughness. Three experimental steels were studied in order to find optimal conditions for the AF formation in the coarse-grained heat-affected zone (CGHAZ). One of the steels was Al-deoxidized, while the other two were Ti-deoxidized. The main focus was to distinguish whether the deoxidation practice affected the AF formation in the simulated CGHAZ. First, two different peak temperatures and prolonged annealing were used to study the prior austenite grain coarsening. Then, the effect of welding heat input was studied by applying three cooling times from 800 °C to 500 °C in a Gleeble thermomechanical simulator. The materials were characterized using electron microscopy, energy-dispersive X-ray spectrometry, and electron backscatter diffraction. The Mn depletion along the matrix-particle interface was modelled and measured. It was found that AF formed in the simulated CGHAZ of one of the Ti-deoxidized steels and its fraction increased with increasing cooling time. In this steel, the inclusions consisted mainly of small (1–4 μm) TiOx-MnS, and the tendency for prior austenite grain coarsening was the highest.