Surface-functionalized -Ga2O3 and diamond substrates were directly bonded by annealing at 250 °C in atmospheric air. Prior to bonding, the -Ga2O3 and diamond surfaces were OH-terminated by oxygen plasma irradiation and H2SO4/H2O2 cleaning, respectively. After contacting the OH-terminated surfaces with each other, direct bonding was formed by a thermal dehydration reaction. The annealed specimen had a shear strength of 14 MPa because of the generation of chemical bonds between -Ga2O3 and diamond surfaces. The analysis of interface structures revealed that the -Ga2O3 and diamond surfaces were atomically bonded without nano-voids, cracks, or any intermediate layer. The β-Ga2O3 and diamond substrates were bonded without any serious loss in crystallinity except for the outermost surfaces. We believe that the -Ga2O3/diamond heterostructure can contribute to the high-power applications of -Ga2O3 devices.
Au–Au surface activated bonding is promising for room-temperature bonding. The use of Ar plasma vs. O2 plasma for pretreatment was investigated for room-temperature wafer-scale Au–Au bonding using ultrathin Au films (<50 nm) in ambient air. The main difference between Ar plasma and O2 plasma is their surface activation mechanism: physical etching and chemical reaction, respectively. Destructive razor blade testing revealed that the bonding strength of samples obtained using Ar plasma treatment was higher than the strength of bulk Si (surface energy of bulk Si: 2.5 J/m2), while that of samples obtained using O2 plasma treatment was low (surface energy: 0.1–0.2 J/m2). X-ray photoelectron spectroscopy analysis revealed that a gold oxide (Au2O3) layer readily formed with O2 plasma treatment, and this layer impeded Au–Au bonding. Thermal desorption spectroscopy analysis revealed that Au2O3 thermally desorbed around 110 °C. Annealing of O2 plasma-treated samples up to 150 °C before bonding increased the bonding strength from 0.1 to 2.5 J/m2 due to Au2O3 decomposition.
Heterojunctions consisting of p-type diamond substrates and thin exfoliated n-type β-Ga2O3 layers were fabricated at a low temperature using a direct-bonding technique. We have fabricated p+-diamond/n-Ga2O3 (p+–n) and p-diamond/n-Ga2O3 (p–n) structures with different B concentrations in diamond. The p+–n heterojunction exhibited Ohmic behavior, resulting from p+-diamond behaving as a metallic layer. As for the p–n heterojunction, it showed clear rectifying action as a conventional bipolar action with a rectifying ratio >108 at ±10 V and leakage current <10−12 A. The ideality factor and barrier height of the p–n heterojunctions were estimated to be 2.7 and 1.5 eV, respectively. Formation of the p–n junction was evidenced by comparing it with the Schottky junction. An energy band diagram of the p–n heterojunctions with staggered (type-II) band alignment was derived based on electrical investigations.
Au-Au surface activated bonding (SAB) using ultrathin Au films is effective for room-temperature pressureless wafer bonding. This paper reports the effect of the film thickness (15–500 nm) and surface roughness (0.3–1.6 nm) on room-temperature pressureless wafer bonding and sealing. The root-mean-square surface roughness and grain size of sputtered Au thin films on Si and glass wafers increased with the film thickness. The bonded area was more than 85% of the total wafer area when the film thickness was 100 nm or less and decreased as the thickness increased. Room-temperature wafer-scale vacuum sealing was achieved when Au thin films with a thickness of 50 nm or less were used. These results suggest that Au-Au SAB using ultrathin Au films is useful in achieving room-temperature wafer-level hermetic and vacuum packaging of microelectromechanical systems and optoelectronic devices.