We investigated the imaging capability of fixed-voltage fundamental wave amplitude difference (fixed-voltage FAD), which is one of the nonlinear ultrasonic phased array imaging techniques, for three-dimensional crack open/closed distribution. We fabricated two fatigue crack specimens with different thicknesses, which were selected to create different open/closed distributions in them. As a result of applying fixed-voltage FAD with mechanical scans to the thick and thin specimens, the difference in the crack open/closed distribution was successfully visualized. The results are in good agreement with fracture mechanics. Thus, it was demonstrated that fixed-voltage FAD is useful not only for nondestructive testing for aging infrastructures but also for the progress in fracture mechanics.
Ultrasonic phased-array (PA) systems have been widely adopted in the field of nondestructive evaluation for material characterization and imaging of internal defects. Whereas many defects exhibit complex three-dimensional structures, most PA systems provide only two-dimensional images. In this Letter, we demonstrate the ability to create high-resolution 3D images of internal defects using a PA system based on a piezoelectric and laser ultrasonic system (PLUS). The PLUS combines a piezoelectric transmitter to insonify the structure to be inspected with a laser Doppler vibrometer to create a matrix array of receiver points without contact. The small size of the laser beam results in an ultra-multiple number of elements on the order of thousands, which is impossible to achieve with a conventional piezoelectric matrix array transducer. An emission from a piezoelectric transmitter compensates for the intrinsically low sensitivity of a laser Doppler vibrometer. After formulating the 3D imaging algorithm of the PLUS, we demonstrate that the PLUS with 4096 receiving points (i.e., 64 × 64 points) achieves high-resolution 3D imaging in a specimen with a flat bottom hole. We also visualize the complex structure of stress corrosion cracking. We believe that the 3D imaging capability of the PLUS may open up new avenues to the accurate evaluation of material strength, the identification of the types of defects, and the elucidation of the mechanisms of defect initiation.
10 June 2019 in Japanese Journal of Applied Physics
Nondestructive evaluation of closed cracks is one of the most challenging issues in ultrasonic testing. Thus far, we have developed a closed crack imaging method, subharmonic phased array for crack evaluation (SPACE) of using only longitudinal (LL) subharmonic waves. In this study, we investigated the imaging capabilities of SPACE with LL and mode-converted shear (LS) subharmonic waves. After formulating the imaging algorithm, this method was applied to a complexly branched stress corrosion crack (SCC). As a result, a few responses of the branched SCC were observed in the LL subharmonic image, whereas more multiple responses of the branched SCC with higher resolutions were observed in the LS subharmonic image. Importantly, the LS subharmonic image successfully visualized a lot of responses that were not visualized in the LL subharmonic image. This suggests that the use of both LL and LS subharmonic images will make SPACE more robust for practical application.
18 August 2022 in International Journal of Hydrogen Energy
The nondestructive inspection of concrete structures is indispensable for ensuring the safety and reliability of aging infrastructures. Ultrasonic waves having a frequency of tens of kHz are frequently used to reduce the scattering attenuation due to coarse aggregates. Such low frequencies enable the measurement of the thickness of concrete structures and detection of layer-type defects, such as delamination, whereas it causes a lack of sensitivity to crack-type defects. In this paper, to realize the ultrasonic phased array (PA) imaging of crack-type defects, we fabricated a low-frequency (LF) array transducer with a center frequency of hundreds of kHz. To avoid the crosstalk between piezoelectric elements and dampen the vibration of each element, we adopted soft lead zirconate titanate (soft PZT) with a low mechanical quality factor. Subsequently, we optimized the geometry of each piezoelectric element using a finite element method to generate a short pulse. After validating the design in a fundamental experiment using a single-element transducer, we fabricated a 32-element array transducer with a center frequency of 350 kHz. To show the imaging capability of the LF array transducer, we applied it to a concrete specimen with a delamination. As a result, the PA with the LF array transducer clearly visualized the delamination, which could not be visualized using the PA with a 2.5 MHz array transducer. Furthermore, we applied it to a more challenging defect, a slit, which is sometimes used to simulate crack-type defects. As a result, the PA with the LF array transducer clearly visualized a slit of 1 mm width and 40 mm height in a concrete specimen. Thus, we demonstrated the usefulness of the LF array transducer for inspecting crack-type defects.