Strain in InGaN/GaN multiple-quantum well (MQW) light emitters was relaxed via nanopatterning using colloidal lithography and top-down plasma etching. Colloidal lithography was performed using Langmuir-Blodgett dip-coating of samples with silica particles (d = 170, 310, 690, 960 nm) and a Cl2/N2 inductively coupled plasma etch to produce nanorod structures. The InGaN/GaN MQW nanorods were characterized using X-ray diffraction (XRD) reciprocal space mapping to quantify the degree of relaxation. A peak relaxation of 32% was achieved for the smallest diameter features tested (120 nm after etching). Power-dependent photoluminescence at 13 K showed blue-shifted quantum well emission upon relaxation, which is attributed to reduction of the inherent piezoelectric field in the III-nitrides. Poisson-Schrödinger simulations of single well structures also predicted increasing spectral blueshift with strain relaxation, in agreement with experiments.
Highly efficient long-wavelength InGaN LEDs have been a research focus in nitride LEDs for their potential applications in displays and solid-state lighting. A key breakthrough has been the use of laterally injected quantum wells via naturally occurring V-defects which promote hole injection through semipolar sidewalls and help to overcome the barriers to carrier injection that plague long wavelength nitride LEDs. In this article, we study V-defect engineered LEDs on (0001) patterned sapphire substrates (PSS) and GaN on (111) Si. V-defects were formed using a 40-period InGaN/GaN superlattice and we report a packaged external quantum efficiency (EQE) of 6.5% for standard 0.1 mm2. LEDs on PSS at 600 nm. We attribute the high EQE in these LEDs to lateral injection via V-defects.
Achieving high quantum efficiency in long-wavelength LEDs has posed a significant challenge to the solid-state lighting and display industries. In this article, we use V-defect engineering as a technique to achieve higher efficiencies in red InGaN LEDs on (111) Si through lateral injection. We investigate the effects of superlattice structure on the V-defect distribution, the electroluminescence properties, and the external quantum efficiency. Increasing the relative thickness of In in the InGaN/GaN superlattice and the total superlattice thickness correlate with a reduction of active region defects and increased external quantum efficiencies. The highest measured on-chip EQE was 0.15% and based on Monte-Carlo ray tracing simulations for light extraction we project this would correspond to a flip-chip EQE of ~2.5%.
Nanoscale light emitting diodes (nanoLEDs, diameter < 1 µm), with active and sacrificial multi-quantum well (MQW) layers epitaxially grown via metal organic chemical vapor deposition, were fabricated and released into solution using a combination of colloidal lithography and photoelectrochemical (PEC) etching of the sacrificial MQW layer. PEC etch conditions were optimized to minimize undercut roughness, and thus limit damage to the active MQW layer. NanoLED emission was blue-shifted ∼10 nm from as-grown (unpatterned) LED material, hinting at strain relaxation in the active InGaN MQW layer. X-ray diffraction also suggests that strain relaxation occurs upon nanopatterning, which likely results in less quantum confined Stark effect. Internal quantum efficiency of the lifted nanoLEDs was estimated at 29% by comparing photoluminescence at 292K and 14K. This work suggests that colloidal lithography, combined with chemical release, could be a viable route to produce solution-processable, high efficiency nanoscale light emitters.
1 January 2017 in Colloids and Surfaces A: Physicochemical and Engineering Aspects