An Al2014-alumina (Al2O3) composite's characteristics are significantly influenced by the reinforcement particle size variation. Therefore, this study examines the microstructure, mechanical, fractography, and wear performance of an Al2014-Al2O3p composite made using a unique two-stage stir casting method and various alumina weight fractions (9, 12, and 15 wt %). Three categories of alumina particle size are used, i.e., fine particle size (FPS, 8 μm), intermediate particle size (IPS, 53 μm), and coarse particle size (CPS, 88 μm). The shapes of the composites were characterized using scanning electron microscopy. According to scanning electron microscopic analyses of the microstructure, the FPS dispersion was more uniform than IPS and CPS, whereas CPS causes agglomeration. Additionally, the studies show that the FPS composite outperformed CPS and IPS composites in terms of mechanical characteristics and wear performance. The fractography study shows conical and equiaxed dimple failure in the Al2014 matrix and the circular cavities.
The present study aims at producing transient liquid phase (TLP) bonded Al2219 joints with pure Cu (copper) as an interlayer. The TLP bonding is carried out at the bonding temperatures in the range of 480 to 520 °C while keeping the bonding pressure (2 MPa) and time (30 min.) constant. Reaction layers are formed at the Al-Cu interface with a significant increase in diffusion depth with the increase in the bonding temperature. The microstructural investigations are carried out using scanning electron microscopy and energy-dispersive spectroscopy. X-ray diffraction study confirms the formation of CuAl2, CuAl, and Cu9Al4 intermetallic compounds across the interface of the bonded specimens. An increase in microhardness is observed across the bonding zone with the increase in the bonding temperature, and a maximum hardness value of 723 Hv is obtained on the diffusion zone of the specimen bonded at 520 °C. Furthermore, the fractography study of the bonded specimens is carried out, and a maximum shear strength of 18.75 MPa is observed on the joints produced at 520 °C.
This study examines the changes in microstructure and mechanical properties of friction stir-welded (FSW) dissimilar joints between AA2014-T6 and AA5052-H32 aluminium alloys, with an emphasis on optimizing tool rotation speed for enhanced joint quality. FSW is performed at three different tool rotation speeds (860, 1160, and 1460 rpm) while maintaining a constant welding speed and tool tilt angle of 40 mm/min and 1°, respectively. The joint created at an optimal rotation speed of 860 rpm exhibits outstanding mechanical properties, with an ultimate tensile strength (UTS) of 211 ± 1.0 MPa, a yield strength of 181 ± 1.5 MPa, and an elongation of 16.1%. The joint efficiency, in comparison to the aluminium alloy AA5052-H32, is 93.8%, indicating minimal strength loss relative to the parent material. Vickers hardness tests across the weld cross-section reveal a maximum hardness of 156 ± 1.5 HV in the stir zone, closely matching the hardness of the stronger AA2014-T6 base metal. Fractographic analysis of the FSW joint made at 860 rpm indicates a predominantly ductile failure mode with micro-dimple fracture surfaces, whereas higher tool rotation speeds exhibit brittle characteristics with circular voids and tear ridges.
8 October 2024 in Fracture and Structural Integrity
Diffusion welding is an advanced joining process that assures the feasibility of joining dissimilar metal alloys without producing metallurgical impurities at the joint interface. Two significant aerospace alloys, AA2219 and Ti-6Al-4V, are diffusion welded for the various holding times (30-120 minutes) by keeping the bonding temperature and pressure constant. The effect of holding time on the microstructure of the diffusion welded joints is evaluated using scanning electron microscopy (SEM), and the diffusion behaviour across the joint interface is ensued by the line scan energy dispersive spectroscopy (EDS). The obtained results show that the hardness across the joint interface is increased with increase in holding time. Furthermore, the maximum shear strength of 143.58 MPa is achieved for the joint formed at the holding time of 90 minutes and reduced thereafter. The formation of a thick intermetallic layer at a higher holding time strongly affects the shear strength. It is evident from the resulting fractured surfaces that the joints predominantly failed at the bonding interface, showcasing the brittle kind of failure. The X-ray diffraction (XRD) study on the fractured surfaces substantiates the formation of AlTi, Al2Ti and Al3Ti intermetallic compounds.