The present study aims to enhance the strength of friction stir lap welded aluminum alloys by using an interlayer of graphene nanoplatelets (GNPs) at the weld interface. With GNP interlayer, the weld strength and percentage elongation increased by 121 and 53%, respectively, as compared to the weld without GNP interlayer. The interlayer also changes the mode of fracture from brittle in the weld without GNP to ductile mode. Grain size in the weld with interlayer decreased by ~38% as equated to the weld without GNP. The height of the hook defect (HD) and cold lap defect (CLD) decreased by 26% and 41%, respectively, in the weld with GNP interlayer as compared to the weld without interlayer. In weld with interlayer, the bottom of the top plate on the retreating side acts as the potential site for fracture due to the presence of an interfacial defect, and undeformed GNP layer. The strengthening of the weld is attributed to various primary strengthening mechanisms like thermal mismatch, grain refinement, Orowan looping, and load transfer. Moreover, GNP interlayer also prevents the formation of the Al2O3 layer at the lap interface and thus contribute significantly in the weld strengthening.
The influence of friction stir processing parameters and the subsequent evolution of microstructures and corrosion behaviour of Al–SiC surface composites fabricated in the presence of graphitic flakes are presented in this paper. The circumferential shear stress exerted by the rotating tool exfoliates the graphite flakes into few-layered graphene during processing. These graphene flakes preferentially occupy both the grain boundaries and the SiC–Al interface during recrystallization. The potentiodynamic polarization test, in 3.5 wt% sodium chloride (NaCl) solution, is conducted for samples processed at various tool rotational speeds and it is found that the presence of this thin graphitic layer at these locations reduces the intergranular and interfacial corrosion to a great extent. The tool rotational speed has a significant influence on processing, and samples fabricated at an optimum tool rotational speed of 2200 rpm shows better corrosion resistance and mechanical properties as compared to that at lower and higher speeds. Raman spectroscopic analysis, X-ray diffraction studies and microhardness tests corroborate the experimental results and the proposed mechanisms.
In the present investigation, friction stir welding (FSW) of a gamma prime (γ′) strengthened Haynes 282 nickel-base superalloy by using a novel hemispherical tool is documented. A joint efficiency of ~ 96% was achieved in the as-welded condition, which further increased to ~ 100% after two-step post-weld aging heat treatment. An extremely fine (~ 2 μm) grained microstructure was observed in the FSWed region compared with the coarse (~ 48 μm) grain base metal region. The carbides (MC and M23C6) and γ′ precipitates are identified as the important microstructural constituent phases observed in the welded region. The aging heat treatment resulted in the precipitation of the γ′ strengthening phase and altered the morphology of the M23C6 carbide phase in the welded region from a continuous film to discrete particles at the grain boundaries. The preliminary results concerning tool life suggest that no significant tool wear occurs at least up to a welding distance of 200 mm. Therefore, the novel hemispherical tool design allows the successful FSW of high-temperature application materials without any significant tool wear or high heat generation.