Laboratory tests are one of the most fundamental and crucial methods in rock mechanics and engineering research. Natural rock specimens are challenging to acquire, and traditional casting methods involve prolonged curing times and cannot produce rock-like specimens with complex internal fractures. Furthermore, 3D printing technologies such as SLA, SLS, and FDM possess inherent limitations. In this study, high-silica sand was used as the printing material, and sand powder 3D printing technology was harnessed to fabricate rock-like specimens. Uniaxial compression tests were performed on specimens with varying placement times, aimed at investigating the impact of placement time on the mechanical properties of sand 3D-printed rock-like specimens. Acoustic emission technology was used to explore the internal state changes during deformation and failure of specimens with different placement times. The findings indicate that the mechanical properties of sand powder 3DP rock-like specimens exhibited no deterioration over time after approximately 7 days of placement. The internal structure remained unchanged across different placement times. This study's outcomes underscore the superiority of sand powder 3D printing technology within the realm of rock mechanics and establish the groundwork for the accurate and efficient fabrication of rock-like specimens through sand powder 3D printing technology in the future.
The size effect has a significant effect on the mechanical behavior of rock, thereby fundamentally influencing the stability of rock excavations. The main challenge associated with the experimental research on the size effect of fractured rock mass lies in the difficulty of specimen preparation to represent the influence of size and fracture on the mechanical behavior of the rock material. In order to preliminarily explore the feasibility of 3D printing technology in the field of rock mechanics, fractured rock specimens of different sizes and different fracture characteristics were produced using sand powder 3D printing technology. The uniaxial compression test was combined with the digital image correlation method (DIC) technology to study the influence of the size effect on the mechanical properties and deformation and failure of different fractured specimens. The research finds that: (1) The elastoplastic mechanical characteristics of the sand powder 3D printed specimens are similar to soft rock. Specimen size and fracture angle have significant effects on the mechanical properties of specimens. Under different fracture conditions, the uniaxial compressive strength (UCS) and Elasticity Modulus of sand powder 3D specimens should be decreased with the increase of the specimen size, and the size effect has different influences on the specimens with different fracture characteristics. (2) Under different fracture conditions, the crack initiation position and failure mode of specimens of various sizes are affected by the fracture inclination to varying degrees. (3) The size effect of fractured rock mass is closely related to the defect level inside the rock mass. The size effect originates from the heterogeneity inside the material. The research results verify the feasibility of applying sand powder 3D printing technology to study the size effect of fractured rock masses and provide an innovative test method for the size effect test study. Preliminary exploration of the size effect of fractured rock masses provides a powerful reference for related research in this field. The study proves the feasibility of applying sand powder 3D printing technology in similar rock mechanics tests and contributes to understanding the size effect of a fractured rock mass.
Numerical testing is an ideal testing method in the research on the mechanical behaviors of jointed rock. However, there are few systematic studies focused on the comparison between the two-dimensional (2D) and the three-dimensional (3D) simulation effects on rock mechanical behaviors, particularly those of jointed rock. In this paper, a particle flow model was established by utilizing PFC2D and PFC3D to represent the rock materials, and the rock (especially jointed rock) mechanical behaviors (uniaxial compressive strength UCS, tensile strength TS, crack initiation stress level Kσ, and the pattern of crack initiation) between 2D and 3D models were compared and analyzed. As expected, the result shows that the UCS and TS showed an increasing tendency with the increase in the joint angle (β) for both the 2D and the 3D models, and the strength of the 3D model was less than that of the 2D model under uniaxial compression but was greater than that of the 2D model under uniaxial tension. The crack initiation and Kσ of the specimens were essentially the same for the 2D and 3D models, and the tensile stresses are more concentrated than the compressive stresses before the failure of the specimen; the uniaxial tensile failure more closely approached abrupt failure than the uniaxial compression failure. The tensile cracks were often initiated at the tips of the joints for both the 2D and 3D models, but they were initiated in the middle of the joints when β was low (β = 0° and β = 15° in both the 2D and 3D models) under uniaxial compression and when β reached 90° under uniaxial tensile. The test results were validated and further analyzed with mathematical analysis. This study has relative referential value to experiments on jointed rock and to analysis of the instability fractures of engineering rock mass.
In the field of rock engineering, tensile failure is one of the most significant failure modes due to the presence of joints/fractures. However, due to the limitations of current laboratory testing, it is difficult to carry out direct tensile tests on jointed rock specimens in the laboratory. To study the effect of joints on the mechanical behavior and failure mode of jointed rock specimens, a three‐point modeling method that can consider arbitrarily arranged rock joints is deduced and applied to discrete element simulation. The effects of different joint angles (the inclination angle α, rotation angle β, and superimposed angle γ of α and β, where γ is the angle between the joint and horizontal plane), the density (n), and the rate of cutting area (RCA) of the specimen loading surface (LSS) on the tensile strength (σt), elastic modulus in tension (Et), and failure mode of the specimens were analyzed. The results show that the joint angle (considering α, β, and γ) and RCA have a significant effect on the resulting σt and failure mode, while n has a significant effect on Et. The failure mode of the specimen changes from tensile failure along the joint to direct tensile failure of the specimen as γ increases, and the mechanical behavior transitions from unstable to stable. In addition, the main influence of γ on the mechanical behavior of specimens is revealed, and the change process of the failure mode after the cutting of the LSS is analyzed. The present research can be utilized for multiple purposes, including the joint development of surrounding rock and failure dominated by tensile failure in underground engineering, especially for tunnels, roadways, chambers, and so forth.
The presence of joints and other types of discontinuities has a significant effect on the mechanical properties of rock, especially for tensile properties to fundamentally influence the stability of rock excavations. The main challenge associated with the experimental research on jointed rock lies in the difficulty to carry out amount of direct tensile tests for analysis of the effect of joint geometric parameters on mechanical properties. In this study, a particle flow model was established by utilizing the flat-joint contact model (FJM) to represent the rock materials. After microscopic parameter calibration, 53 sets of the numerical model were used for investigating the relationship between jointed geometric parameters and tensile mechanical properties. The results show that the crack initiation is related to trace length and joint angle , and the tensile-shear crack will appear as increase. The uniaxial tension strength and had first a weak negative correlation and then a positive correlation as the increases, which was consistent with mathematical calculations. Furthermore, the relative importance (RI) analysis showed that the plays a decisive role among the joint geometric parameters for affecting , and the effect factors of were joint angle , length , density , and aperture in that order. The present research can be utilized for multiple purposes in the field of jointed rock engineering, such as prediction of surrounding rock instability analysis and estimating the variable values in the inversion analysis in practical engineering projects.
In order to understand the mechanism of some unconventional failures such as rockburst caused by deep rock excavation, the failure characteristics of burst-prone sandstone specimens under static and dynamic loads were studied by using the MTS816 rock mechanics testing system and the split Hopkinson pressure bar (SHPB) experimental system, as well as the effects of bedding angle and impact pressure on rock mechanical properties and failure patterns. The uniaxial compression test used a cylindrical specimen with a height of 50 mm and a diameter of 100 mm, and cylindrical specimens with height and diameter of 50 mm were adopted in the SHPB tests. The bedding angles in the tests are 0°, 45°, and 90°. In the dynamic impact test, three different impact pressures were applied to observe the magnitude of impact load on the mechanical behaviors of the burst-prone sandstone specimens. The results show that with the increase in the bedding angle, the uniaxial compressive strength firstly decreases and then increases. When the bedding angle is 45°, the uniaxial compressive strength is the lowest. The uniaxial compressive strength is highest when the bedding angle is 0°. The burst-prone sandstone specimens with different bedding angles had three different failure pattern types. Under the dynamic loading, the stress-strain curves show springback phenomenon; with the increase in impact pressure, the dynamic strength of the burst-prone sandstone specimens with each bedding angle increases; the fracture degree of the bedding sandstone specimens gradually increases. The dynamic strength of the 45° burst-prone sandstone specimen is the lowest, and it has the highest fracture degree.