The corrosion resistance of FeCoNiCr high-entropy alloy deposits was investigated upon being prepared by current electrodeposition. The coatings were co-deposited in an electrolyte of an aqueous ferrous, cobalt, nickel, and chromium sulfates solution. Energy dispersive spectrometry analysis demonstrated that all four elements were co-deposited successfully. At the same time, the results from SEM indicate that the surface of the coating exhibits a granular morphology, with uniform density and no presence of cracks, with sizes ranging from 500 nm to 5 μm. Furthermore, X-ray diffraction patterns enunciated that the as-deposited coatings were amorphous. The polarization curves of the FeCoNiCr high-entropy alloy coating were measured by an electrochemical workstation in 3.5 wt.% NaCl, 1 mol·L−1 H2SO4 and 1 mol·L−1 NaOH solutions. The results revealed that the coating exhibited excellent corrosion resistance. The corrosion mechanism of the FeCoNiCr high-entropy alloy coating was analyzed in different environments. Moreover, the scratch testing method was employed to determine the alloy adhesion on the substrate, with higher values obtained for the FeCoNiCr alloy.
Employing atomic force microscopy (AFM) to measure passive film thickness on stainless steel (SS) in aqueous solution is proposed. SUS304 austenite and SUS329J4L duplex SS samples partly covered by gold were set in a minicell. To remove the original film, the SS surface but gold was etched using dilute sulfuric acid. After cleaning, open circuit potential (OCP), and distance from the sample surface to the top of the gold were measured. They were then immersed in either 1.0% NaCl; 5.0% NaCl; or aqueous solution with pH ranging from 1.0 to 10.0 and measured again. Differences between the first and subsequent measures of OCP suggested a passive film had formed in solution with pH ranging from 2.8 to 10.0. Similarly, differences among AFM measures revealed the observed film thickness increased with increase in pH and with decrease in chloride ions. Also, film thickness in water was greater than that in a vacuum. Comparison of AFM measurements of passive film on the austenite and sigma phases in sensitized SUS329J4L duplex SS revealed the film was thinner on the sigma phase containing more chromium. Taken together, these findings suggest the proposed method is applicable for measuring the thickness of passive films in aqueous solution.
13 March 2018 in Corrosion Engineering, Science and Technology: The International Journal of Corrosion Processes and Corrosion Control
Sigma phase generally precipitates in duplex stainless steel during slow cooling, which usually causes loss in both corrosion resistance and fracture toughness. To develop a non-destructive method to detect the sigma phase in duplex stainless steel for in situ use in the quality management of large structures, the double-loop electrochemical potentiokinetic reactivation behaviour of continuously cooled duplex stainless steel SUS329J4L at different cooling rates was investigated under different conditions. The polarisation condition with the solution of 0.5 M H2SO4 + 0.01 M KSCN + 0.5 M NaCl and the potential scanning rate of 0.83 mV s−1 were determined as suitable and sensitive. This paper is part of a supplementary issue from the 17th Asia-Pacific Corrosion Control Conference (APCCC-17).