Chengde chromium-bearing vanadium–titanium magnetite (CCVTM) has been used as an important mineral resource in sinter making. The MgO content of this sinter can be enhanced by adding dolomite, which improved operation of the blast furnace. The effects of MgO in the form of dolomite on metallurgical properties, microstructure and mineral compositions of CCVTM sinter were studied by a sinter pot test, X-Ray Diffraction (XRD), Scanning Electron Microscope (SEM), and mineral phase microanalysis. The results were as follows: The flame front speed and sinter coefficient decreased with an increase in MgO content from 2.66 to 3.86% by adding dolomite. With an increase in MgO content from 2.66 to 3.86%, the flame front speed, sintering utilization factor, and the value of RI decreased, while RDI and the softening–melting properties improved. In addition, the value of sinter strength (TI) reached a maximum value at MgO = 3.56%. In addition, an increase in the abundance of magnetite, magnesium ferrite, and silicate phase, as well as a decrease in hematite, was found with an increase in MgO content. We concluded that the most appropriate MgO content in the sinter is 3.56%.
The sintering pot test was used to investigate the effect of TiO2 on the sintering behavior of chromium-bearing vanadium–titanium magnetite (CVTM) sinter. The main characterization methods of X-ray fluorescence (XRF), X-ray diffraction (XRD), scanning electron microscopy-energy disperse spectroscopy (SEM-EDS), and metallographic microscopy were employed. In this study, yield, tumbler index (TI), vertical sintering speed, productivity, reduction degradation index (RDI), and reduction index (RI) were tested and calculated. The yield first increases from 82.87% to 84.37% and then decreases to 83.65%, vertical sintering speed first increases from 17.00 mm·min−1 to 23.45 mm·min−1 and then decreases to 20.61 mm·min−1, and productivity first increases from 2.33 t·m−2·h−1 to 3.14 t·m−2·h−1 and then decreases to 2.69 t·m−2·h−1 with increasing TiO2 content. The TI increases from 45.81% to 52.09%, and RDI increases from 74.99% to 96.74%, while RI decreases from 67.92% to 47.15% with increasing TiO2 content.
High-chromium vanadium and titanium magnetite (HCVTM) sinter has poor properties. The coke ratio has an important effect on the behavior of HCVTM sintering as it affects the mineral phases in the high-chromium vanadium and titanium sinter (HCVTS) via changing the sintering temperature and atmosphere. In this work, the sintering behavior of HCVTM mixed with varying coke ratios was investigated through sintering pot tests, X-ray diffraction (XRD), gas chromatographic analysis, and mineral phase analysis. The results show that, with the increase of the coke ratio from 4.0% to 6.0%, leading to the increase of the combustion ratio of the flue gas, the vertical sintering rate and sinter productivity decrease. Meanwhile, with the change of the coke ratio, the content of magnetite, silicate, and perovskite increase, while the hematite and calcium ferrite decrease. In addition, the tumble strength and reduction ability of HCVTS decrease, and its degradation strength increase. It was found that the appropriate coke ratio for the sintering process was 5.0 wt %.
This study discusses the oxidation induration and swelling behavior of chromium-bearing vanadium titanomagnetite pellets (CVTP) with Co2O3 additions. The reduction swelling index (RSI) and compressive strength of reduced CVTP (CSRC) were investigated with simulated coke oven gas (COG). The results show that the compressive strength (CS) of CVTP decreases from 2448 to 1983 N and the porosity of CVTP increases from 14.86 to 22.49% with increasing Co2O3 additions. The Co2O3 mainly exists in the form of CoFe2O4 in both of CVTP and reduced CVTP, and the CoFe2O4 is hard to be reduced by thermodynamic calculation. The Co-bearing phase mainly distributes on gap edges and among adjacent hematite grains. Many cracks and pores distribute along the grain boundaries and damage the connection of hematite grains. The CSRC decreases from 901 to 376 N, and RSI of reduced CVTP increases from 5.87 to 9.05% with increasing Co2O3 additions. The Co2O3 addition facilitates the aggregation and diffusion of metallic iron particles, and the aggregations of metallic iron thicken the lamellar crystals. The pores and interval of grains enlarge with increasing Co2O3 additions. This study can supply the theoretical and technical basis for the utilization of CVTP and waste residue-bearing cobalt with COG recyclable technology.