Objectives: The aim of this study is to assess the micro-tensile bond strength and the mode of failure of a bioactive hybrid self-adhesive composite (Surefil one) under various dentin conditions. Methods: Thirty-two extracted human molar teeth were used to test the micro-tensile bond strength of Surefil one under different dentine conditions (no treatment, 37% phosphoric acid etching, and universal adhesive) in comparison with a resin-modified glass ionomer (RIVA). All restorations were light cure-bonded onto flat dentine and then sectioned into beams. Then, fractured specimens were observed under a light microscope to evaluate the mode of failure. Results: The Surefil one no-treatment group (NTG) exhibited the highest micro-tensile bond strength. Furthermore, there was no statistically significant difference observed between the Surefil one adhesive group (EAG) and the Surefil one acid etch group (EG). However, compared to other groups, the resin-modified glass ionomer (RIVA) produced the lowest results, which are statistically significant. Conclusion: Surefil one offers superior bond strength values when compared to resin-modified glass ionomers. Furthermore, Surefil one requires no dentin condition and has more straightforward clinical steps.
The aim of this study was to evaluate the mechanical properties (flexural strength (FS), flexural modulus (FM), Vickers microhardness (VMN), and shear bond strength (SBS)) of preheated composites. Two preheated composites (Z350XT and Proclinic) and one self-adhesive resin cement (RelyX™ U200) were used to fabricate specimens. All the specimens were subjected to thermocycling before their mechanical properties were evaluated. One-way ANOVA was used for statistical analysis, followed by Tukey’s post hoc test. The chi-square test was used to evaluate the failure modes after SBS test. Results: RelyX™ U200 had a significantly higher FS (106.22 ± 14.23 MPa) than Proclinic (85.76 ± 12.75 MPa) and Z350 (71.47 ± 22.98 MPa). Z350 (118.10 ± 11.3 GPa) and RelyX™ U200 (110.88 ± 13.44 GPa) had significantly higher FMs than Proclinic (83.72 ± 9.3 GPa). A significantly higher VHN was seen with Z350 (136.84 ± 11.52 VHN) compared to Proclinic (115.25 ± 17.15 VHN) and RelyX™ U200 (100.83 ± 12.69 VHN). Z350 had a higher SBS (20.75 ± 5.6 MPa) than RelyX™ U200 (15.4 ± 3.46 MPa), while Proclinic was the weakest among all the groups (6.76 ± 1.44 MPa). In the failure mode analysis, the mixed failure mode was predominantly seen in all groups. In conclusion, not all preheated composites behave the same and it is the clinician’s responsibility to select the appropriate material for every clinical situation.
This in vitro study evaluated and compared the shear bond strength (SBS) of three restorative materials bonded to dentin: a glass hybrid ionomer (EQUIA Forte HT), a resin-modified glass ionomer (RIVA Light Cure), and a nanofilled composite resin (Filtek Z350 XT). Additionally, their modes of failure were assessed. Thirty extracted human teeth were prepared and randomly assigned to three groups (n = 10) by restorative material: Group 1: Filtek Z350 XT; Group 2: EQUIA Forte HT; Group 3: RIVA Light Cure. All materials were applied following manufacturer instructions. SBS testing used a universal testing machine, applying a load at the tooth–restoration interface at 1 mm/min until failure. SBS values were recorded in megapascals (MPa). Failure modes were examined under a stereomicroscope at 40× magnification. A one-way ANOVA compared mean SBS among groups, with post hoc tests for pairwise group comparisons. Results: Filtek Z350 XT had the highest mean SBS (21 MPa), followed by RIVA Light Cure (7.5 MPa) and EQUIA Forte HT (7.2 MPa). One-way ANOVA indicated a statistically significant difference in SBS (p < 0.05). Post hoc analysis showed Filtek Z350 XT had significantly higher SBS than the glass ionomer-based materials, while EQUIA Forte HT and RIVA Light Cure did not differ significantly. Conclusions: Filtek Z350 XT demonstrated significantly higher shear bond strength to dentin than the glass ionomer-based materials. No significant SBS difference was found between the resin-modified and hybrid glass ionomers.