One of the primary challenges in the automotive industry is the wear of engine components, such as the crankshaft and camshaft, which is the most pronounced during the engine’s startup phase, when the amount of lubricant fluid is at its lowest. This study aims to enhance the surface wear resistance of automotive crankshaft steel by applying a boriding thermochemical process. This process forms a hard surface layer on the steel, improving its mechanical properties and bolstering its wear resistance, especially under dry conditions. Boride layers were achieved using the powder-pack boriding process in a conventional furnace, with meticulous treatment times of 2, 4, and 6 h at a constant temperature of 950 °C. The nature of the layers was analyzed using X-ray diffraction, and their tribological behavior was evaluated using the pin-on-disk test. The growth of the layers was directly proportional to the treatment time and was estimated at 145 µm and 48 µm for the 6 and 2 h of treatment, respectively. The surface hardness increased from 320 HV for the non-treated steel to 2034 HV for the sample exposed to 950 °C for 6 h. The results indicate a significant reduction in the coefficient of friction from 0.43 for the non-treated steel to 0.12 for the samples exposed to 950 °C for 6 h, suggesting potential wear protection during the engine starting period.
Boriding is a thermochemical process that improves the surface properties of metallic materials, such as wear resistance, hardness, and Young’s modulus. The current work evaluated the kinetics of boride layers formed by boriding on AISI H13 steel. The AISI H13 steel samples were covered with a non-commercial powder mixture of 70% wt. SiC, 20% B4C wt. and 10% wt. KBF4. The samples were treated for 2, 4, and 6 h at 850, 875, and 900 °C, respectively. The growth kinetics of boride layers were estimated as a function of the treatment parameters, using a solution of the second Fick’s Law, as in a parabolic model. Also, the hardness of layers was assessed by Vickers microindentation. Optical examination of the samples showed a biphasic FeB/Fe2B layer at all temperatures after 6 h of treatment. In contrast, those exposed for 2 h exhibited a monophasic Fe2B layer with isolated zones of the FeB phase in all temperatures. The results suggested that the obtained layer thicknesses are highly dependent on the treatment parameters. After 2 h at 850 °C, the samples exhibited a well-defined layer with a thickness of 8.51 ± 1.01 μm, whereas after 6 h it was 24.39 ± 1.01 μm. The activation energy was estimated at 230.63 kJ/mol, with a correlation coefficient (R2) of 0.97, consistent with values reported in the literature. Additionally, the hardness values were estimated to range from 1880 to 2192 HV for the FeB phase and from 1294 to 1715 HV for the Fe2B phase, indicating that the hardness of the boride layers is highly dependent on the treatment conditions.
The boriding process was applied to generate hard layers on three different steels—AISI 1018, AISI 316L stainless steel, and AISI 4340 crankshaft steel—with varying treatment times and temperatures (2, 4, and 6 h, and 900, 950, and 1000 °C). X-ray diffraction analyses were performed to characterize the phases formed in the coatings. Microscopy techniques were used to evaluate the morphology and thickness of the layers. In addition, micro- and nanoscale mechanical tests were performed to determine changes in the structural and functional properties of the steel. These steels, due to their nature, are subject to wear processes under operating conditions. Therefore, coating these steels with a hard layer that exhibits better properties could help them withstand the working conditions. The boride layers formed on the different steels exhibited varying morphologies. On the one hand, layers with a strong saw-toothed morphology formed on AISI 1018 steel.,On the other hand, extremely flat layers were observed on AISI 316L stainless steel, and, finally, layers with a moderate front of growth were obtained on AISI 4340 crankshaft steel. The results indicated that not only were the layers' morphologies different, but also their chemical composition and mechanical properties changed. The layers obtained on AISI 1018 and the 4340 crankshaft steel were of monophasic Fe2B nature with an 8.83% wt. of boron content, while the nature of those obtained on AISI 316L stainless steel was biphasic FeB/Fe2B, with a 16.23% wt. of boron content. This compositional difference gives the layers different properties. The higher boron content gives the biphasic layers the highest hardness but also makes them more brittle than the monophasic layers. Therefore, it is essential to assess the characteristics of the resulting layers in relation to a specific application.