Highly dispersed MnOx–CeO2 and MnOx–ZrO2–CeO2 catalysts for the carbon monoxide oxidation reaction are synthesized. Using the XRF and the XRD methods, the formation of the Mn–Ce–O and the Mn–Zr–Ce–O solid solutions, as well as the presence of Mn2O3 and Mn3O4, is established. The specific surface area of the synthesized materials is 121 and 155 m2/g, respectively, the particle size being equal to 8–10 nm. The X-ray photoelectron (XPS) spectra is deconvolved and the relative content of the ionic forms of Mn, the lattice oxygen Oα, and the high-energy forms Oβ are determined. Upon studying the thermal stability of catalysts, it is established that the two-component systems have low thermal stability, causing the particle size to increase to 32 nm, the specific surface area to decrease to 29 m2/g, and thus the catalytic activity to deteriorate. For MnOx–ZrO2–CeO2, less significant changes take place: the particle size is 27 nm, the specific surface area is 43 m2/g, and thus its catalytic activity is higher than that for MnOx–CeO2. Investigation of the state of the components of the near-surface layer of catalysts after isothermal aging makes it possible to ascertain the change in content of ionic forms of Mn, Oα, and Oβ. It is concluded that doping of the two-component MnOx–CeO2 systems with the Zr4+ ions is expedient. The resulting ZrO2–MnOx–CeO2 solid solution is more resistant to high temperatures.
Nanodispersed SnO2–CeO2 catalysts for the oxidation of CO and СН4 were synthesized by coprecipitation in a water–isopropanol solution followed by thermal treatment. It was shown that SnхCe1–хO2 solid solutions based on the crystal lattice of cerium dioxide were formed at x ≤ 0.15. The samples were characterized by energy dispersive spectroscopy (EDS), X-ray diffraction (XRD) analysis, transmission electron microscopy (TEM), nitrogen adsorption–desorption, and gas chromatography. The materials had a mesoporous structure: the specific surface area was 52.3–69.7 m2/g, and the total pore volume was 0.073–0.108 cm3/g. When the SnO2 content was greater than 30 mol %, plate-shaped SnO2 particles with sizes greater than 100 nm were formed along with nearly spherical solid solution particles of size 8–10 nm. The synthesized solid solutions were highly active in the oxidation reactions of CO and methane, and they can be used as catalysts and supports.
We have synthesized Au/MnOx–CeO2 nanocatalysts for the low-temperature oxidation of carbon monoxide. Gold nanoparticles applied by the deposition precipitation (DP) method were used as an active phase. The composition, structure, and textural characteristics of the materials and the charge state of the components of the catalysts were studied using X-ray diffraction, X-ray photoelectron spectroscopy, highresolution transmission electron microscopy, inductively coupled plasma mass spectrometry, and low-temperature nitrogen adsorption measurements. The carbon monoxide concentration in the catalytic oxidation products was determined by gas chromatography. The influence of calcination temperature on the charge state of the components of the surface layer of Au/ MnOx–CeO2 and the catalytic activity of the materials was examined. The catalytic activity of the materials was shown to be determined to a significant degree by the Mn3+, Au3+, and weakly bound oxygen concentrations in the surface layer.
The nanodisperse Au/Cе0.72Zr0.18Pr0.1O2catalysts for low-temperature oxidation of carbon monoxide were synthesized. The compounds were identified by XRD, XPS, TEM, ISP-MS, and gas chromatography....