Titanium and titanium alloys such as Ti-6Al-4V are generally considered as difficult-to-machine materials. This is mainly due to their high chemical reactivity, poor thermal conductivity, and high strength, which is maintained at elevated temperatures. As a result, the cutting tool is exposed to rather extreme contact conditions resulting in plastic deformation and wear. In the present work, the mechanisms behind the crater and flank wear of uncoated cemented carbide inserts in the turning of Ti6Al4V are characterized using high-resolution scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDS), and high-resolution Auger electron spectroscopy (AES).The results show that, for combinations of low cutting speeds and feeds, crater and flank wear were found to be controlled by an attrition wear mechanism, while for combinations of medium to high cutting speeds and feeds, a diffusion wear mechanism was found to control the wear. For the latter combinations, high-resolution SEM and AES analysis reveal the formation of an approximately 100 nm thick carbon-depleted tungsten carbide (WC)-layer at the cemented carbide/Ti6Al4V interface due to the diffusion of carbon into the adhered build-up layers of work material on the rake and flank surfaces.
Using Ti6Al4V as a work material, a methodology to systematically investigate the diffusion degradation of cemented carbide during machining is proposed. The methodology includes surface characterization of as-tested worn inserts, wet etched worn inserts, metallographic cross-sectioned worn inserts as well as the back-side of the produced chips. Characterization techniques used include scanning electron microscopy (SEM), energy dispersive X-ray spectroscopy (EDS), Auger electron spectroscopy (AES) and time of flight secondary ion mass spectroscopy (ToF-SIMS). The results show that the characterization of wet etched worn inserts gives quick and useful information regarding the diffusion degradation of cemented carbide, in the present work the formation of a fine crystalline W layer (carbon depleted WC layer) at the tool-work material interface. The present study also illuminates the potential of AES analysis when it comes to analyzing the degradation of cemented carbide in contact with the work material during machining. The high surface sensitivity in combination with high lateral resolution makes it possible to analyze the worn cemented carbide surface on a sub-µm level. Especially AES sputter depth profiling, resulting in detailed information of variations in chemical composition across interfaces, is a powerful tool when it comes to understanding diffusion wear. Finally, the present work illustrates the importance of analyzing not only the worn tool but also the produced chips. An accurate characterization of the back-side of the chips will give important information regarding the wear mechanisms taking place at the tool rake face–chip interface. Surface analysis techniques such as AES and ToF-SIMS are well suited for this type of surface characterization.
CVD α-Al2O3 coatings on cemented carbides are widely used in steel turning, where cutting tool performance is strongly dependent on the crystallographic texture of the α-Al2O3 layer. Residual stress, cooling-crack density, and hardness are key factors influencing coating integrity during machining. Although texture has been reported to affect these properties, trends remain inconsistent in the literature. In this work, three CVD α-Al2O3/Ti(C,N) coatings with identical architecture, substrate, and processing route, but distinct α-Al2O3 textures: i. c-plane (0001) , ii. r-plane (01-12) , and iii. a-plane (11-20) were investigated to isolate the role of texture under controlled conditions. The (0001) coating exhibited the highest tensile residual stress and the lowest crack density, while the (01-12) and (11-20) coatings showed lower stresses and denser crack network. This behaviour is consistent with a texture-dependent thermal expansion mismatch, complemented by orientation-dependent stress accommodation during cooling. The (01-12) and (11-20) textures, with a greater in-plane contribution of the c-axis, develop higher intrinsic thermal stress and thus promote more extensive crack formation for stress relaxation compared to texture. Nanohardness values were comparable across the three textures. The results demonstrate that α-Al2O3 texture has a clear influence on residual stress and cracking, but a limited effect on hardness. These findings provide a more consistent basis for interpreting texture–property relationships and suggest that the performance of (0001)-textured coatings in steel turning is primarily associated with reduced crack density and their response under directional loading, rather than with differences in hardness.
Notch wear in austenitic stainless steel turning develops rapidly and remains a key productivity limitation with carbide tools. This work identifies the initiation mechanism of notch wear when turning EN 1.4307 stainless steel using CVD-coated cemented carbide inserts with an Al2O3 top layer. Turning tests were performed under dry conditions, followed by optical wear measurements and chip surface analysis. The tool–chip interface chemistry and material transfer were characterized using SEM/EDS, while high-frequency acoustic emissions were recorded to resolve the dynamics of adhesive events. Thermo-mechanical FEM simulations were conducted to map contact pressure and temperature along the cutting edge. The results show that adhesive wear initiates immediately at engagement and governs notch formation: polluted SiO2 deposits act as an active bonding medium, and repeated bond formation/rupture removes extremely thin flakes of tool and coating material, evidenced by Al2O3 and Ti(C,N) fragments on the chip and by characteristic acoustic cluster waves. A new tool–chip contact model is presented, indicating that high pressure and high temperature within the polluted SiO2 near the chip’s outmost side promote larger, stronger adhesive bonds together with the absence of ceramic particles near the rake in the notch area. Oxidation and diffusion are assumed to be secondary processes that become relevant after local coating loss, while adhesion remains the primary removal mechanism during early and intermediate stages.