As-doped polycrystalline ZnTe layers grown by metalorganic chemical vapor deposition (MOCVD) have been investigated as a back contact for CdTe solar cells. While undoped ZnTe films were essentially insulating, the doped layers showed significant rise in conductivity with increasing As concentration. High p-type carrier densities up 4.5 × 1018 cm−3 was measured by the Hall-effect in heavily doped ZnTe:As films, displaying electrical properties comparable to epitaxial ZnTe single crystalline thin films in the literature. Device incorporation with as-deposited ZnTe:As yielded lower photovoltaic (PV) performance compared to reference devices, due to losses in the open-circuit potential (VOC) and fill factor (FF) related to reducing p-type doping density (NA) in the absorber layer. Some minor recovery observed in absorber doping following a Cl-free post–ZnTe:As deposition anneal in hydrogen at 420 °C contributed to a slight improvement in VOC and NA, highlighting the significance of back contact activation. A mild CdCl2 activation process on the ZnTe:As back contact layer via a sacrificial CdS cap layer has been assessed to suppress Zn losses, which occur in the case of standard CdCl2 anneal treatments (CHT) via formation of volatile ZnCl2. The CdS sacrificial cap was effective in minimising the Zn loss. Compared to untreated and non-capped, mild CHT processed ZnTe:As back contacted devices, mild CHT with a CdS barrier showed the highest recovery in absorber doping and an ~10 mV gain in VOC, with the best cell efficiency approaching the baseline devices.
1 October 2021 in Solar Energy Materials and Solar Cells
In-situ Cd-saturated growth of polycrystalline CdTe:As thin film was performed by metal organic chemical vapour deposition at a low temperature of 350 °C, to investigate the impact on As doping and device VOC. Device characterization showed conversion efficiency of ∼14%, and VOC of 772 mV, which is an improvement to the baseline device with CdTe:As absorber layer grown at 390 °C under non-saturated conditions. When the low temperature Cd-saturated growth was combined with chlorine heat treatment at a higher temperature of 440 °C (in contrast with the standard 420 °C) for 10 min, device efficiency improved to ∼17% with a high VOC of 877 mV. As a result, ∼100 mV boost in VOC from baseline is demonstrated with Cd-saturated CdTe:As device. Micro-photoluminescence and time-resolved photoluminescence measurements performed on these Cd-saturated CdTe:As devices confirmed that minority carrier lifetime significantly improved.
CdTe solar cells were produced using metal organic chemical vapour deposition (MOCVD), which employed a (Zn,Al)S (AZS) high resistant transparent (HRT) layer at the transparent conducting oxide (TCO)/Cd(Zn)S emitter interface, to enable the higher annealing temperature of 440 °C to be employed in the chlorine heat treatment (CHT) process. The AZS HRT remained intact with conformal coverage over the TCO after performing the high CHT annealing, confirmed by cross-section scanning transmission electron microscopy coupled with energy-dispersive X-ray spectroscopy (STEM-EDX) characterisation, which also revealed the Cd(Zn)S emitter layer having been consumed by the CdTe absorber via interdiffusion. The more aggressive CHT resulted in large CdTe grains. The combination of AZS HRT and aggressive CHT increased open circuit voltage (Voc) and improved solar cell performance.
21 January 2025 in Solar Energy Materials and Solar Cells