This study investigated the effect of silane and surfactant treatments of graphene nanoplatelets (GnPs) on the mechanical and thermal properties of silicone rubber (SR) composites. GnPs were modified with aminopropyltriethoxysilane (APTES), vinyltrimethoxysilane (VTMS), and Triton X-100, and then the pristine GnPs and functionalized GnPs were individually incorporated into the SR. Compared with the pristine GnP/SR composite, the composites reinforced with modified GnP showed better tensile strength, elongation at break, and thermal conductivity properties due to better dispersion of modified GnPs and stronger interfacial interactions between the modified GnPs and matrix. The mechanical properties and thermal conductivity of the VTMS-GnP/SR composite were comparable to the properties of the Triton-GnP counterpart, but better than that of the APTES-GnP/SR composite. In addition, the VTMS-GnP/SR composite demonstrated the highest thermal stability and crystallization temperature among the four types of composites. The remarkable improvement of mechanical and thermal properties of the VTMS-GnP/SR composite was mainly due to the covalent linkage of VTMS-GnP with SR. The VTMS treatment was a more appropriate modification of GnP particles to improve the multifunctional properties of SR.
Ceramifiable silicone rubber composites play important roles in the field of thermal protection systems (TPS) for rocket motor cases due to their advantages. Ceramifiable silicone rubber composites filled with different contents of ZrSi2 were prepared in this paper. The fffects of ZrSi2 on the vulcanization, mechanical and ablation resistance properties of the composites were also investigated. The results showed that the introduction of ZrSi2 decreased the vulcanization time of silicone rubber. FTIR spectra showed that ZrSi2 did not participate in reactions of the functional groups of silicone rubber. With the increasing content of ZrSi2, the tensile strength increased first and then decreased. The elongation at break decreased and the permanent deformation increased gradually. The thermal conductivity of the composite increased from 0.553 W/(m·K) to 0.694 W/(m·K) as the content of the ZrSi2 increased from 0 to 40 phr. In addition, the thermal conductivity of the composite decreased with the increase of temperature. Moreover, thermal analysis showed that the addition of ZrSi2 increased the initial decomposition temperature of the composite, but had little effect on the peak decomposition temperature in nitrogen. However, the thermal decomposition temperature of the composite in air was lower than that in nitrogen. The addition of ZrSi2 decreased the linear and mass ablation rate, which improved the ablative resistance of the composite. With the ZrSi2 content of 30 phr, the linear and mass ablation rate were 0.041 mm/s and 0.029 g/s, decreasing by 57.5% and 46.3% compared with the composite without ZrSi2, respectively. Consequently, the ceramifiable silicone rubber composite filled with ZrSi2 is very promising for TPS.
Carbon fiber fabric-reinforced phenolic resin composites are widely used as thermal protection materials for thermal protection systems in hypersonic vehicles and capsules. In this work, carbon fiber fabric-reinforced boron phenolic resin composites modified with MoSi2 and B4C were prepared via a compression molding technique. The high-temperature performance of the composites as well as the oxidation behavior of the carbon fibers was studied. The results indicate that the incorporation of B4C improves the performance of composites at high temperatures. The residual weight rate of composites with 15 phr B4C (BP-15) sufficiently increased from 23.03% to 32.91% compared with the composites without B4C (BP-0). After being treated at 1400 °C for 15 min, the flexural strength of BP-15 increased by 17.79% compared with BP-0. Compared with BP-0, the line ablation rate and mass ablation rate of BP-15 were reduced by 53.96% and 1.56%, respectively. In addition, MoSi2 and B4C particles had a positive effect on the oxidation of carbon fibers in the composites. After treatment at 1400 °C, the diameter of the as-received carbon fiber was reduced by 31.68%, while the diameter of the carbon fiber in BP-0 and BP-15 decreased by 15.12% and 6.14%, respectively. At high temperatures, the liquid B2O3 from B4C and MoSi2-derived complex-phase ceramics (MoB, MoB2, Mo2C, Mo4.8Si3C0.6) acted as an oxygen barrier, effectively mitigating the oxidation degree of the carbon fibers.
Montmorillonite (MMT) was added to silicone rubber (SR) to improve the ablation resistance of the silicone. Following this, different quantities of silicon carbide whiskers (SiCw) were incorporated into the MMT/SR to yield a hybrid, ablative composite. The tensile strength and elongation at break of the composite increased after the addition of MMT. The ablation test results showed that MMT helped to form a covering layer by bonding with the silica and other components on the ablated surface. The linear and mass ablation rates exhibited decreases of 22.5% and 18.2%, respectively, in comparison to a control sample. After further incorporation of SiCw as the second filler, the resulting composites exhibited significantly higher tensile strength and ablation resistance, but not particularly lower elongation at break in comparison to the control sample. The SiCw/MMT fillers were beneficial in forming a dense and compact covering layer that delayed the heat and oxygen diffusion into the inner layers, which improved the ablation properties effectively. The remaining whiskers acted as a micro skeleton to maintain the composite’s char strength. Compared to the control sample, the linear and mass ablation rates of the composite after incorporating 6 phr SiCw and 10 phr MMT decreased by 59.2% and 43.6%, respectively. These experimental results showed that the fabricated composites exhibited outstanding mechanical properties and excellent ablation resistance.