Objective: The study aims to evaluate the wear surface using 3D surface roughness and other material characterization of zirconia fabricated using photopolymerization based Lithography-based Ceramic Manufacturing (LCM). Method: LCM technology was used to fabricate zirconia specimens of size 10 × 10 × 2mm3. Scanning Electron Microscope, 3D–profilometer, X-ray Diffraction, and hardness test characterized the samples before and after wear and Coefficient of friction (COF) was monitored. Result: The COF was around 0.7 and did not differ much between the horizontally and vertically printed specimens. However, the surface roughness after wear for horizontally printed specimen was 0.567 ± 0.139 μm, while that for vertically printed specimen was 0.379 ± 0.080 μm. The reduced valley depth and the dale void volume were low for the vertically printed zirconia specimen, indicating lesser voids and low fluid retention. In addition, it was observed that the hardness value of the vertically printed sample was better. The scanning electron microscopic images and 3D surface profiles of the zirconia specimens depicted the surface topography and revealed the wear track. Conclusion: The study shows that zirconia fabricated using LCM technology possesses surface roughness of about 0.5 μm with no machining scars that are usually associated with CAD/CAM dentistry and also indicating agreement with clinically acceptable values for minimal surface roughness of dental restorations. Dental restorations using LCM fabricated zirconia redues the requirement of post-processing work flow that is part of CAD/CAM dentistry.
Objective: To investigate the effect on zirconia surface of the post-fabrication surface treatments on the morphological characteristics and mechanical properties of CAD/CAM milled dental zirconia specimens as well as to identify the critical parameters in the measurement of oral retention under in vitro circumstances. Method: The zirconia specimens (N = 20, n = 4) were subjected to CAD/CAM milling and divided into five groups. The specifications were: Group G1—sintered; Group G2—sintered followed by a polishing process; Group G3—sintered followed by polishing and sandblasting with alumina particles Al2O3 (110 µm); Group G4—sintered followed by sandblasting; Group G5—sintered followed by sandblasting with polishing as the end process. All the groups were subjected to Fretting wear tests, 3-D surface roughness measurements, and Vickers’s Micro hardness tests. Investigation of the phase transformation using XRD, and surface feature examination using SEM were also carried out. Additionally, one-way ANOVA, Tukey, and Pearson correlations were statistically analysed. Results: The fabrication processes had a significant effect on the performance of zirconia specimens in all the groups (p > 0.05). Specimens that underwent polishing as the last process exhibited lower surface roughness. The monoclinic phase of zirconia was observed in all the specimens before and after wear except for those in the G2 and G5 groups, where polishing was the end process. In G5, the post-wear surface properties revealed lower surface roughness and hardness. Further, the SEM and 3-D topography show grooves as seen by the dale void volume (Vvv) values; shallow valley depth (Svk); micro craters; and wear track. Conclusion: Specimens in G5 that were subjected to multistep post-fabrication process, namely sandblasting followed by polishing, yielded better results when compared to those in the other groups (G1, G2, G3, and G4). G5 with an interlayer of alumina is recommended for clinical applications due to its enhanced surface properties, mechanical properties, and low wear.