In this work, the stir casting method was applied to obtain composites based on the alloy AN EW 6061 used as a metal base, and Al2O3 particles as a reinforcement. Composites play a significant role as engineering materials. Therefore, it is necessary to study, in detail, the production methods and the factors that affect their mechanical properties. For this purpose, we have carried out a planned experiment wi ASM International th the aim to use regression analysis to predict the influence of particle size and mass fraction on hardness of the obtained composites. The full factorial experimental design with two factors was used, which was analyzed at three levels. Hardness was observed as a system response, while particle size and mass fraction were set as influencing factors. Influencing factors were observed at three levels: 50, 80 and 110 ?m for the particle size and 2, 5 and 8 mass%. Measured hardness values of the composites ranged from 72 HV10 to 80 HV10. Based on the probability values (p<0.05), it was determined which factors are important for the system response. Statistical analysis has shown that linear terms of the influence factors (size and mass fraction of reinforcement particles) and the square term of the mass fraction have statistical significance on the hardness change. The square term of the particle size and the interaction term of the influencing parameters do not have a statistically significant contribution in predicting the hardness value. Thus, a second-order polynomial model was obtained by the regression analysis. Influence of input factors on the system response and the adequacy of the obtained mathematical model were determined by using the Analysis of Variance (ANOVA). Based on the statistical data analysis, it was established that, the particle mass fraction has a greater influence on hardness of the obtained composite in relation to the particle size. By comparing the experimental and predicted values, a high degree of agreement was achieved so that the chosen model of the factorial experiment was adequate (R2=0.989). It can be also concluded that the developed regression model can be applied to predict hardness of the aluminum composite reinforced by Al2O3 particles in the chosen variation interval of particle size and mass fraction.
22 December 2025 in Archives of Metallurgy and Materials
In this study, various contents of graphene nanosheets (GNS) were successfully incorporated into Sn-0.7Cu base alloy by powder metallurgy (PM) technique to form Sn-0.7Cu-xGNS composite materials. The synthesis process included mixing and mechanical alloying, compacting and sintering. The effects of GNS on the microstructure, wettability, microhardness and melting properties were investigated. Optical and scanning electron microscopy (SEM) with energy-dispersive spectroscopy (EDS) revealed that the distribution of GNS in the solder matrix became more evident as the content of GNS increased. The reinforcement particles were homogeneously distributed at the grain boundaries, resulting in a finer β-Sn structure. The melting temperatures of the synthesized composites, determined by differential scanning calorimetry (DSC), are slightly higher than those of the Sn-0.7Cu base alloy. Incorporating GNS into the Sn-0.7Cu matrix enhanced microhardness up to 15.65% and reduced the contact angle between the composite solder and copper substrate up to 48.6%, significantly improving wettability.
The increasing demand for environmentally friendly electronic materials has encouraged the development of lead-free solder alloys and sustainable production technologies. Despite numerous alternatives, the eutectic Sn-0.7Cu alloy has been recognized as a promising candidate for lead-free solder applications due to its low cost, acceptable mechanical properties, and compliance with RoHS and WEEE regulations. This study investigates the effect of graphene nanoparticles, in the form of graphene nanosheets (GNS), on the microstructural and mechanical properties of Sn-0.7Cu matrix composites produced via powder metallurgy. GNS was incorporated into the matrix in small weight fractions (0, 0.02, 0.04, 0.06, 0.08, and 0.10 wt.%) to promote microstructural refinement and enhance the mechanical properties of the composites. Optical microscopy was used to characterize the microstructure of the sintered samples, while microhardness was measured using the Vickers method. The results indicate that increasing the graphene content significantly refines the grains, reducing the average grain size by approximately 54 % and increasing the microhardness by about 16 % compared to the base alloy.
This paper presents the study of microstructural changes and microhardness of the martensitic b' phase during aging of the nickel-aluminum bronze (NAB) with the nominal composition CuAl9Ni3Fe3. After casting, the alloy was annealed at 900˚C for 2 h followed by a rapid cooling in cold water. The quenched samples were aged at 350°C and 450°C for 10 min, 60 min, 180 min, and 600 min. After each stage of heat treatment, the microhardness values of the martensitic b' phase were studies, and the microstructure was analyzed using the SEM microscopy with the EDS. The microhardness of b' martensite increased during the aging due to the precipitation of the nano c phase rich in nickel.
Development of various types the so-called "environmentally friendly" solders has been extensively investigated worldwide as an alternative to the lead-based solders. This study investigated the impact of graphene nanoparticles on microstructure and thermal properties of the lead-free solders. The nanocomposite solders were produced using the powder metallurgy method. The graphene nanoparticles were used as the reinforcement in the form of graphene nanosheets (GNS). The microstructural analysis showed that the GNS particles were homogeneously distributed along the grain boundaries, resulting in a refined b-Sn structure. At room temperature, density was measured using the Archimedes method, while the thermal diffusivity was determined using the flash method. The thermal conductivity of the Sn-0.7Cu nanocomposite solders was calculated using a fundamental equation. Increasing the GNS content up to 0.08 wt% in the Sn-0.7Cu solder matrix led to a slight decrease in density of the nanocomposite solders compared to the base solder, while the highest thermal conductivity was achieved with a 0.05 wt% GNS addition, reaching 44.74 Wm⁻¹ K⁻¹.
The aim of this work is to analyze the process of obtaining and thermal treatment on the grain size of copper microalloyed with iron and phosphorus (0,003 wt%Fe i 0,014 wt%P). Microalloyed copper was obtained in two ways: by melting cathode copper and prealloys CuFe0,1 and CuP6,42 in an induction furnace followed by the casting of the same raw materials and the up-casting process, followed by extrusion. The samples obtained in this way were subjected to thermomechanical treatment, which involved cold plastic deformation by rolling with 70% reduction, followed by annealing at 470°C for 80 minutes. Based on the microphotographs and the ImageJ software, the average grain size and grain size distribution were determined for each tested sample. The results showed that the average grain size of the extruded sample was smaller, and the microstructure was more uniform and had a higher degree of recrystallization, which can be attributed to severe plastic deformation (extrusion).