This study addresses the dielectric performance of nonpolar hydrocarbon liquids and mineral oils under negative polarity stress. Stopping length for non-breakdown streamers, breakdown voltages and velocities for various pre-breakdown streamer modes have been studied for a selection of model liquids (cyclohexane and white oils), for a gas to liquid oil, and a refined naphthenic transformer oil. Studies of propagation modes were done using an 80 mm point to plane gap and a step voltage with 0.5 μs rise time. Light emission and pre-breakdown currents have been recorded and instantaneous velocities have been derived from images of propagating streamers. Compared to positive polarity, there are less differences in streamer behaviour in the oils examined under negative polarity. Breakdown voltages and acceleration voltages are higher for negative streamers than for positive ones, while their propagation velocities are lower. While propagation modes for positive voltages are quite distinct, the mode changes for negative ones are more gradual. The behaviour of both positive and negative streamers is in line with the hypothesis that the propagation is governed by electron avalanches and quantum chemical properties of liquid components.
13 March 2024 in IEEE Transactions on Dielectrics and Electrical Insulation
This paper describes measurements of conduction currents in both neat and commercial insulating liquids. Conduction in thermodynamic equilibrium has been measured by applying a low ac voltage in a uniform field. High-field pre-discharge currents have been measured in a needle-to-plane configuration stressed with respectively high voltage ac and steep step high voltage pulses. There was significantly increased conduction for high field compared to low field conditions. Notably, measurements at high fields in needle-plane configurations indicate space charge limitation of currents with polarity differences. The high field conduction exhibited considerable variation across different liquids. At high applied fields, electronic processes are probably governing the charge formation. Simulations indicate that space charges may reduce the local field in front of needle tips at time scales relevant for propagating streamers.
Propagation of positive streamers in dielectric liquids, modeled by the electron avalanche mechanism, is simulated in a needle–plane gap. The streamer is modeled as an RC-circuit where the channel is a resistor and the extremities of the streamer have a capacitance towards the plane. The addition of the RC-model introduces a time constant to the propagation model. Increase in capacitance as a streamer branch propagates reduces its potential, while conduction through the streamer channel increases its potential, as a function of the time constant of the RC-system. Streamer branching also increases the capacitance and decreases the potential of the branches. If the electric field within the streamer channel exceeds a threshold, a breakdown occurs in the channel, and the potential of the streamer is equalized with the needle electrode. This is interpreted as a re-illumination. According to this model, a low conductive streamer branch can propagate some distance before its potential is reduced to below the propagation threshold, and then the RC time constant controls the streamer propagation speed. Channel breakdowns, or re-illuminations, are less frequent when the channels are conductive and more frequent for more branched streamers.
9 May 2022 in IEEE Transactions on Dielectrics and Electrical Insulation
Changing the current loading of mass-impregnated non-draining power cables causes the pressure in the insulation to vary over a wide range. It is generally recognized that under certain conditions—typically after a large load reduction—the pressure becomes so low that shrinkage cavities (voids) form in the insulation, and that partial discharges that may damage the insulation ignite. A finite element model for temperature, electric field and pressure dynamics throughout the insulation layer has been developed. Comparisons with previously obtained measurements on full-scale HVDC subsea cable samples subjected to a variety of loading patterns, external pressures (sea depths) and ambient temperatures, show that the model replicates the pressure behavior of the insulation reasonably well. Most importantly, the complicated viscoelastic properties of the lead sheath, which have a profound effect on the internal pressure dynamics and thereby on the prospects of forming potentially harmful cavities, appear to be sufficiently accurately modelled.
9 February 2023 in IEEE Transactions on Dielectrics and Electrical Insulation
Polyetheretherketone (PEEK) is commonly used in power connectors due to its excellent mechanical and electrical properties. In submarine electrical components, water molecules can diffuse through polymeric sealings and interfaces and finally increase the humidity in the main electrical insulation system. To examine the effect of water sorption on the dielectric properties of a semi-crystalline commercially available PEEK, polarization and depolarization currents were measured on samples preconditioned in a climate chamber to either a dry state or to a water concentration of 5000 ppmw at 30, 60 and 90 °C. The water absorption process was characterized and found to follow Fick’s law, with the solubility decreasing with increasing temperature. The absorption of water was found to strongly increase the electrical conductivity. At 90 °C the conductivity increased by 85 times compared to the value measured on dry conditioned samples. The conductivity of dry PEEK also increases less with temperature than that of wet PEEK, indicating a lower activation energy in the absence of water molecules. The conduction mechanism in wet PEEK insulation is likely ionic hopping.
Scanning electron Microscopy (SEM) coupled with energy dispersive X-ray analysis (EDX) were used for qualitative and quantitative trace element analysis of inception sites of vented water-trees in a modern HV XLPE cable aged in salt water. The aim of this paper is to examine different methodologies based on SEM/EDX to identify localized high concentrations of ions responsible for the initiation and growth of vented water trees. Long vented water trees were observed initiated at the insulation and conductor screens with lengths larger than $600 \mu\mathrm{m}$ after 4 months of ageing at 500 Hz. The initial results presented in this paper indicate that measurements at the sample sub-surface only, are likely not sufficient to reliably detect the ions causing vented water treeing. The FIB - milling technique showed to be a promising technique.