Key Lab for Robot and Welding Automation of Jiangxi Province, Mechanical and Electrical Engineering School, Nanchang University, Nanchang 330031, China
Auto-generated profile, based on publicly available information
Guanpeng Liu
Key Lab for Robot and Welding Automation of Jiangxi Province, Mechanical and Electrical Engineering School, Nanchang University, Nanchang 330031, China
The microstructure and mechanical properties of Al/Cu ultrasonic welding joints were investigated. Results show that: (i) the joint strength increased when the welding time increased within a certain range, and a maximal resistant force of 163.04 N was obtained when the welding duration and welding static pressure were 200 ms and 7.2 MPa, respectively; (ii) with a further increase of welding time, the bonding interface was gradually occupied by a thick strip layer of brittle Al2Cu (θ2) phase, thus decreasing the strength; (iii) the maximum temperature in the welding region was 360 °C during the welding process, and a recrystallization phenomenon was identified near the welding interface; (iv) the average nanohardness of Cu, the Cu-Al interfacial reaction layer and Al were 1.04 GPa, 1.34 GPa, and 0.53 GPa, respectively, which is consistent with the formation of the intermetallic compound identified by energy-dispersive X-ray spectroscopy (EDS) and XRD analysis.
1 February 2022 in Journal of Materials Science & Technology
The wetting kinetics of nickel-based filler metal (BNi2) over selective laser-melted Ti-6Al-4V (SLMed TC4) titanium alloy in a protective argon atmosphere is experimentally investigated using a real-time in situ hot stage equipped with an optical microscope. The spreading processes at different temperatures are similar, and the overall wetting/spreading process can be roughly divided into three stages: (i) an initial stage, (ii) a rapid spreading stage, and (iii) an asymptotic stage. Moreover, the wetting kinetics of the BNi2/SLMed TC4 system can be expressed by empirical power exponential function Rn~t with n = ~1. In the process of spreading, Ti-based solid solution (Ti(ss)) and intermetallic compound (Ti2Ni and TiB2) were formed at the interface within the reaction domain, and the phase transition of α’ martensitic to α-Ti and β-Ti also took place. The influence of elevated temperature on the spreading and wetting kinetics of the BNi2/SLMed TC4 system was studied, and the results show that the increase of temperature has a slightly promoting effect on the spreading, but a limited impact on the value of n. In addition, the spreading and wetting kinetics of BNi2/SLMed TC4 system are similar to those of BNi2 on conventional forged TC4 substrate.
A typical dissolution wetting system, Bi-Sn eutectic filler metal over a Bi substrate in a high-purity argon atmosphere was investigated first using real-time in situ hot stage microscopy for the extensive use of the sharp-interface model and the diffuse-interface model in the modeling of brazing/soldering related wetting systems. Subsequently, the similarities and differences between the aforementioned models in describing the issues of the wetting and spreading interfaces were discussed in terms of soldering definition and theoretical formula derivation. It is noted that (i) the mutual dissolution diffusion between the liquid Bi-Sn solder and Bi substrate were obvious. As a result, the composition and volume of the liquid solder is constantly changing during the wetting and spreading process; (ii) the sharp-interface model is a special case of the diffuse-interface model of the Cahn-Hilliard nonlinear diffuse-equation under the convective dominant condition; (iii) although there are differences between the sharp-interface model and the diffuse-interface model, both of them could be used in brazing/soldering related processes; and, (iv) the agreement between the experimental and simulation results of the sharp-interface model is not as good as that of the diffuse-interface model, which can be attributed to the effects of the elements’ diffusion and the phase transformation.