Recent advancements in β-Ga2O3 materials’ growth and device developments are briefly reviewed with the focus on low-pressure chemical vapor deposition (LPCVD) of β-Ga2O3. β-Ga2O3 films are grown on off-axis c-sapphire and (010) β-Ga2O3 substrates via high-temperature LPCVD (HT-LPCVD) with growth temperatures ranging between 950 and 1050 °C. The effects of HT-LPCVD growth conditions on material properties are comprehensively studied. With relatively higher growth temperatures, an increased O2 flow rate is required to maintain β-Ga2O3 crystalline quality with high electron mobility. The growth rate of the HT-LPCVD β-Ga2O3 film scales with the increase of growth temperature and O2 flow rate. The film growth rate is strongly related to the sapphire substrate off-axis angle, which determines the preferred nucleation sites from the step edges. The transport properties of samples grown on substrates with different off-axis angles are compared. The optimized growth temperature for obtaining films with high electron mobility varies with the off-axis angle. From this comprehensive study, high-quality β-Ga2O3 films grown on c-sapphire are achieved with room temperature mobilities of 126 cm2/V s (6° off-axis c-sapphire), 116 cm2/V s (8° off-axis c-sapphire), and 119 cm2/V s (10° off-axis c-sapphire) at carrier concentrations of mid-1016 cm−3. β-Ga2O3 LPCVD homoepitaxy optimized at elevated growth temperatures is performed on Fe-doped semi-insulating (010) Ga2O3 substrates. With controllable Si doping, record-high room temperature mobilities of 156 cm2/V s (150 cm2/V s) are achieved with doping concentrations of 3 × 1016 cm−3 (1.5 × 1017 cm−3) at a growth temperature of 1050 °C. Secondary ion mass spectroscopy analysis shows more than an order of magnitude reduction of C and H impurity incorporation with increased growth temperature. Results from this work demonstrate that HT-LPCVD growth is a promising method to produce high-quality β-Ga2O3 films on both off-axis c-sapphire and native Ga2O3 substrates with a fast growth rate and superior transport properties critical for high power device applications.
Unintentional impurity incorporation in GaN drift layers represents a challenging issue that can limit their potential performance in vertical power devices. In this paper, we focus on studying the origins of Fe impurity incorporation in metal-organic chemical vapor deposition (MOCVD) grown GaN materials. Acting as a compensator in n-type GaN drift layers, Fe impurities can reduce the electron mobility in GaN and limit the lowest controllable doping level. Two sources, the sample cleaning process and growth susceptor, were identified as the main mechanisms of Fe incorporation in the MOCVD GaN growth process. It was found that solvent cleaning of the wafer can introduce significant Fe contamination at the growth interface, which would slowly be incorporated into the GaN epilayer, thus causing background Fe impurity as high as 1017 cm−3 level. Moreover, the Fe impurity in the coating material on the susceptor can introduce additional Fe impurity during the growth process. Our studies revealed that the Fe impurity level could be significantly suppressed by more than two orders when an alternative cleaning process was used and the susceptor surface was fully covered by substrates. Characterization of the Fe impurity concentrations was performed via secondary ion mass spectrometry. The trap level (EC − 0.57) eV from deep-level transient spectroscopy that had previously been attributed to Fe confirmed the carrier compensation effect from Fe. Room temperature Hall mobility as high as 1007 cm2/V s was achieved on the MOCVD grown low-Fe GaN. Results from this work will provide guidance for achieving high purity GaN toward high performance GaN vertical power devices.
High power vertical GaN devices are in great demand recently due to their potential on extremely high-power conversion efficiency. Here, we show vertical GaN p–n power diodes fabricated on bulk GaN substrates with an optimized guard ring structure for electrical field management and high breakdown voltage. By using a low doped (∼1015 cm−3) 28 μm thick drift layer in combination with optimized ohmic contacts, a breakdown voltage (VB) of 4.9 kV and a low specific on-resistance (RON) of 0.9 mΩ cm2 were achieved. In combination with the high breakdown voltage and low specific on-resistance, the device demonstrated a Baliga figure of merit (V2B/RON) of 27 GW/cm2.
20 July 2020 in IEEE Transactions on Electron Devices
We demonstrate edge termination for vertical GaN p-n diodes using step-etched triple-zone junction termination extension (JTE). The technique was found to yield high breakdown efficiency without degradation of forward characteristics. The electric field distribution at various JTE thicknesses was simulated, and the experimental results were well matched to the simulation results. The fabricated GaN p-n diode with step-etched triple-zone JTE shows a breakdown voltage of 550 V corresponding to a junction termination efficiency of 75%, with a turn-on voltage of 3.1 V, a specific ON-resistance of 1.3 $\text{m}\Omega \cdot $ cm 2 , and leakage current at −200 V of 80 nA/cm 2 . The multistep JTE strategy demonstration could be important for future applications for multikilovolt-class GaN vertical power devices.
1 September 2020 in Sensors and Actuators A: Physical
A complete set of all optical phonon modes predicted by symmetry for bixbyite structure indium oxide is reported here from a combination of far-infrared and infrared spectroscopic ellipsometry, as well as first principles calculations. Dielectric function spectra measured on high quality, marginally electrically conductive melt grown single bulk crystals are obtained on a wavelength-by-wavelength (also known as point-by-point) basis and by numerical reduction of a subtle free charge carrier Drude model contribution. A four-parameter semi-quantum model is applied to determine all 16 pairs of infrared-active transverse and longitudinal optical phonon modes, including the high-frequency dielectric constant, . The Lyddane–Sachs–Teller relation then gives access to the static dielectric constant, . All experimental results are in excellent agreement with our density functional theory calculations and with previously reported values, where existent. We also perform optical Hall effect measurements and determine for the unintentionally doped -type sample a free electron density of , a mobility of /(Vs), and an effective mass parameter of . Density and mobility parameters compare very well with the results of electrical Hall effect measurements. Our effective mass parameter, which is measured independently of any other experimental technique, represents the bottom curvature of the point in in agreement with previous extrapolations. We use terahertz spectroscopic ellipsometry to measure the quasi-static response of , and our model validates the static dielectric constant obtained from the Lyddane–Sachs–Teller relation.