We implemented invisibility criterion and black–white contrast orientation analysis into low-tilt electron channeling contrast imaging (ECCI) for dislocation-type discrimination in GaN and AlGaN layers grown on a Si(111) substrate. Our ECCI and x-ray diffraction (XRD) analysis attained consistent threading dislocation densities for GaN and AlGaN grown on Si, but demonstrated drastic discrepancy in the percentage of edge-type dislocations, potentially due to the lack of appropriate consideration of mixed-type dislocations in XRD. Further ECCI analysis of GaN/AlGaN heterointerface revealed mixed-type dislocation half-loops and dislocation bending due to compressive strain relaxation, validating that not all the dislocations originated from the mosaic or columnar structure. As a result, XRD analysis based on the mosaic block model does not give reliable edge-to-screw dislocation ratio. The observation of classic van der Merwe–Matthews-type dislocation half-loop nucleation and dislocation gliding could be associated with potential GaN/AlGaN optoelectronic device degradation issues.
Sc-alloyed AlN epilayers were grown on commercial GaN/sapphire templates by molecular beam epitaxy (MBE) to validate the Sc composition of 18% and in-plane lattice matching with GaN. As-grown Sc0.18Al0.82N/GaN heterostructure exhibits a two-dimensional electron gas (2DEG) density of 3.58 × 1013 (2.96 × 1013) cm−2 and a mobility of 241 (295) cm2⋅V−1⋅s−1 at 300 (77) K, demonstrating the feasibility of employing its high spontaneous polarization toward high 2DEG density and highlighting detrimental impurity scattering due to the regrowth interface. Implementation of AlN impurity blocking layers boosts 2DEG mobility to 1290 (8730) cm2 V−1⋅s−1at 300 (77) K. In addition, we have engineered a surface-treatment strategy to selectively decompose the 2.5-nm-thick GaN cap layer of commercial GaN(2.5 nm)/Al0.20Ga0.80N(22 nm)/GaN heterostructure epi-wafers at high temperature prior to MBE regrowth of Sc0.18Al0.82N to eliminate impurity incorporation at the regrowth interface. Regrowth of a Sc0.18Al0.82N layer on the pristine Al0.20Ga0.80N surface increases 2DEG density from 7.89 × 1012 to 9.57 × 1012 cm−2, together with a slight reduction in mobility from 2160 to 1970 cm2⋅V−1⋅s−1 at 300 K, reducing the sheet resistance by 10%. Our calculation implies that it is practical to boost 2DEG density to over 2.0 × 1013 cm−2 by thinning Al0.20Ga0.80N down to 4 nm.
We attain N-polar and Al-polar AlN thin films on Si(111) substrates by plasma-assisted molecular beam epitaxy. The polarity of AlN epilayers has been validated by wet chemical etching using tetramethylammonium hydroxide and by the direct cross-sectional observation of atomic stacking under high-angle annular dark-field scanning transmission electron microscopy. For the 290 nm-thick as-grown N-polar AlN epilayer, x-ray diffraction (XRD) (002) and (102) ω rocking curve peak full width half maximums (FWHMs) are 475 and 1177 arcsec, and the surface mean square roughness (RMS) is 0.30 nm. We flipped the polarity using the metal-flux-modulation-epitaxy (MME) strategy. The MME strategy promotes anti-phase boundaries (APBs) on the {22¯01} crystalline planes instead of commonly observed lateral planar APBs in AlN epilayers. Merging of the tilted APBs at ∼50 nm leads to a complete Al-polar surface. For the 180 nm-thick Al-polar AlN epilayer, XRD (002) and (102) peak FWHMs are 1505 and 2380 arcsec, and the surface RMS is 1.41 nm. Strain analysis by XRD and Raman spectroscopy indicates a uniform tensile strain of 0.160% across the N-polar AlN epilayer surface and a strain distribution of 0.113%–1.16% through the epilayer. In contrast, the Al-polar AlN epilayer exhibits a much broader tensile strain distribution of 0.482%–2.406% along the growth direction, potentially due to the interaction of polarity inversion and strain relaxation.