B4C–TiB2 composite ceramics with ultra-high fracture toughness were successfully prepared via spark plasma sintering (SPS) at 1900 °C using B4C and Ti3SiC2 as raw materials. The results showed that compared with pure B4C ceramics sintered by SPS, the hardness of B4C–TiB2 composite ceramics was decreased, but the flexural strength and fracture toughness were significantly improved; the fracture toughness especially was greatly improved. When the content of Ti3SiC2 was 30 vol.%, the B4C–TiB2 composite ceramic had the best comprehensive mechanical properties: hardness, bending strength and fracture toughness were 27.28 GPa, 405.11 MPa and 18.94 MPa·m1/2, respectively. The fracture mode of the B4C–TiB2 composite ceramics was a mixture of transgranular fracture and intergranular fracture. Two main reasons for the ultra-high fracture toughness were the existence of lamellar graphite at the grain boundary, and the formation of a three-dimensional interpenetrating network covering the whole composite.
Tantalum carbide (TaC) is widely used in aerospace thermal protection due to its high melting point and excellent high-temperature mechanical properties. Conventional solid-phase carbothermal reduction for TaC powders preparation suffers from high reaction temperature, large particle size, and low purity. While tantalum alkoxide complex precursors offer improvements, challenges such as limited crosslinking sites and lack of molecular-level mixing of Ta and C sources remain. To solve these issues, this study synthesized an unsaturated tantalum alkoxide monomer PTC-Pentene using TaCl5 and 1-penten-3-ol as the Ta source and allyl-modified linear phenolic resin as the C source. C=C bonds served as crosslinking active centers during copolymerization to form a dense crosslinked network and resolve insufficient crosslinking sites, while also enabling covalent bonding between Ta source and C source to achieve uniform molecular-level mixing. Analysis of the precursor's carbothermal reduction kinetics revealed that the process occurs in two stages: the 930~1255℃ range controlled by 1.5-order chemical reactions, and the 1255~1400℃ range jointly controlled by 3D diffusion and phase-boundary reactions. By optimizing the C source addition ratio (m(AN):m(TaCl5) =0.6) and pyrolysis conditions (1400℃ for 2 h), TaC powders with an average particle size of 140 nm and an oxygen content of 0.40 wt% were obtained. Using these powders, TaC ceramics were fabricated via SPS process, and their oxyacetylene ablation mechanism was analyzed. The results showed that the Ta2O5 melt resisted O diffusion but was eroded by gas flow. High temperatures caused thermal cracking, while molten Ta2O5 filled the cracks.
Purpose: A continuous chemical vapor deposition (CVD) method has been used to fabricate pyro-carbon (PyC) coating on continuous silicon carbide (SiC) fibers. The paper aims to evaluate these coated fibers by testing filament tensile and using microstructure characterization.Design/methodology/approach: The continuous SiC fiber-reinforced SiC matrix (SiC/SiC) composite is widely studied in aerospace and nuclear applications. The PyC is the probable option in fusion and fast reactor. However, the conventional fabrication method of PyC coating has some drawbacks influencing performance and efficiency.Findings: The results showed that PyC-coated SiC fibers with continuous CVD method are more straight than conventional ones and residual deformations could not be observed, and these PyC coatings have complete geometry and uniform thickness. In different process conditions, the thickness of PyC coating could control from ∼100 to ∼1,000 nm.Originality/value: The coated SiC fibers in a lower gas ratio (1:7 to 1:3), lower pressure (500–1,000 Pa) and appropriate winding speed (3 to 5 rpm) have relative high filament tensile strength (∼3.5 to ∼3.9 GPa). And the strength of coated SiC fibers has a negative correlation with the measured thickness of PyC coating. A distinctive growth process was discovered in the continuous CVD method. In a certain range, the quicker growing rate of PyC is obtained in shorter deposition time which means an efficient and quality method could be applied to fabricate coatings.