In this study, novel findings were obtained regarding the influence of current intensity and electrode distance on the growth of the FeB-Fe2B layer during pulsed-DC powder pack boriding (PDCPB). Boride layer formation was carried out on AISI 1018 and AISI 4140 steels at 900 °C for 2700 s, considering current intensities ranging from 2.5 to 7.5 A and electrode distances of 10, 15, and 20 mm for each current intensity. The growth of the FeB-Fe2B layer was enhanced as the current intensity/electrode distance increased. This was related to the contribution of electromigration, the amount of powder mixture (used during the PDCPB) between electrodes, and Joule heating. Analysis of variance was performed on borided steels to assess the impact of the current intensity/electrode distance on the boride layer growth. The results revealed weight coefficients of approximately 50% for current intensity, around 40% for electrode distance, and a combined contribution of both variables of no more than 3.5%. Finally, multiple regression analyses were conducted to estimate boride layer thickness expressions as a function of the independent variables. The model results demonstrated a 5% error when compared to the experimental boride layer thickness.
17 July 2024 in Journal of Vacuum Science & Technology A
In this study, novel findings were obtained regarding the influence of a 10 A current intensity on the growth of an FeB–Fe2B layer during pulsed-DC powder-pack boriding. Boride layer formation was carried out on AISI 316 L steel at 1123–1223 K for different exposure times at each temperature, considering 10 s polarity inversion cycles. The boride layer was characterized by x-ray diffraction and high-speed Berkovich nanoindentation, the latter being used to determine the hardness and reduced Young’s modulus mappings along the depth of the layer-substrate system. Moreover, the growth kinetics of the FeB–Fe2B layer on the steel’s surface was modeled using the heat balance integral method (HBIM). This involved transforming Fick’s second law into ordinary differential equations over time, assuming a quadratic boron concentration profile in space to determine the B diffusion coefficients in FeB and Fe2B, respectively. From the Arrhenius relationship, the B activation energies in the boride layer were estimated considering the contribution of the electromigration effect; the results showed an approximately 30% reduction compared to the values obtained in the conventional powder-pack boriding for AISI 316 L steel. Finally, the theoretical layer thickness obtained by the HBIM demonstrated an error of no more than 5% against the experimental FeB and FeB + Fe2B layer thickness values.
Ultrafast boriding (UFB) has emerged as an electrically assisted thermochemical surface treatment capable of producing boride layers within remarkably short processing times. In this study, a comprehensive microstructural, kinetic, and mechanistic analysis of boride layer formation on AISI 1045 and AISI 316L steels treated by UFB is presented. Boriding treatments were conducted at different temperatures and exposure times using molten borax as a fully liquid electrolyte under a direct-current electric field. Layer growth was quantitatively described using a mass balance model, enabling the estimation of B diffusion coefficients and activation energies for both FeB and Fe2B layers. The results demonstrate that boride layer growth under UFB is governed by a combined electrochemical-diffusional mechanism, in which electrolysis-driven boron dissociation and electrolysis within a fully molten medium enhance B availability and directed transport toward the substrate. A comparative epistemological analysis reveals that the physical state of the boriding medium plays a decisive role in defining the activation energies and operational efficiency of electrically assisted boriding processes. These findings provide a mechanistic framework for understanding fast boriding and support the rational design of energy-efficient surface treatments.
15 October 2026 in Journal of Vacuum Science & Technology A
This study investigates the application of pulsed-DC powder-pack boriding (PDCPB) to AISI H13 steel using a novel h-graphite-containing powder mixture (GIS-T), as well as the effect of a subsequent double-tempering treatment. Microstructural and chemical analyses by scanning electron microscopy, energy-dispersive X-ray spectroscopy, and x-ray diffraction revealed the preferential formation of Fe2B, with partial suppression of the brittle FeB. The as-borided condition exhibited practical adhesion values almost three times higher than those reported for conventionally borided AISI H13 steel with comparable ceramic layer thickness. Double tempering promoted a thinner boride layer and encouraged the dissolution of the diffusion zone; despite the reduced thickness, the borided + double-tempered condition increased the load-bearing capacity before delamination by 12% compared with the as-borided condition and achieved adhesion values slightly higher than those reported for conventionally borided steels. Using TiN coatings deposited by Physical Vapor Deposition on AISI H13 steel as an industrial benchmark, both PDCPB-treated conditions exhibited practical adhesion values approximately twice as high as those reported for this widely used automotive forming-tool coating.